Flame-retardant cycloolefin copolymer composite material and preparation method thereof

By adding porous molecular sieve or its boric acid modification to the cycloolefin copolymer as flame retardant synergist, combined with the expanded flame retardant, the heat release and flue gas problems during combustion of the cycloolefin copolymer are solved, and its limits are significantly improved Oxygen index and flame retardant properties.

CN118931082APending Publication Date: 2024-11-12NINGXIA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310519013.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Cycloolefin copolymers release a large amount of heat and smoke during combustion, and have a low limit oxygen index, which limits its application and promotion.

Method used

Porous molecular sieve or boric acid modified porous molecular sieve is used as flame retardant synergist, and a cycloolefin copolymer matrix is ​​added to the expanded flame retardant to form a flame retardant composite material, which is prepared by melt blending.

Benefits of technology

The limit oxygen index is increased by 100%, and the peak heat release value of the cone calorimetry test is reduced by 75%, which significantly improves the flame retardant performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931082A_ABST
    Figure CN118931082A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flame retardance of high polymer materials, in particular to a flame-retardant cyclic olefin copolymer (COC) composite material and a preparation method thereof. The invention provides a flame-retardant cycloolefin copolymer composite material. The composite material comprises the following raw materials in parts by weight: 70-80 parts of a cycloolefin copolymer, 20-30 parts of a flame retardant and 0.1-5 parts of a flame-retardant synergist, wherein the flame-retardant synergist is a porous molecular sieve or a modified substance obtained by modifying the porous molecular sieve with boric acid. The porous molecular sieve or the porous molecular sieve modified by boric acid is used as a flame-retardant synergist, and the flame-retardant synergist and an intumescent flame retardant are added into a COC matrix to form the COC flame-retardant composite material. The limit oxygen index of the obtained COC composite material can reach 28%, and the heat release peak value of the obtained COC composite material is reduced by 75% compared with that of COC in a cone calorimetry test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardant polymer materials, in particular to a flame retardant cyclic olefin copolymer composite material and a preparation method thereof. Background Art

[0002] Cyclic olefin copolymer (COC) is a type of high-value-added thermoplastic engineering plastic formed by the copolymerization of cyclic olefin monomers and α-olefins. Unlike traditional polyolefins with low transparency, COC has high heat resistance and high transparency, and is widely used in optical devices, capacitor films, medicine, engineering plastics and other fields.

[0003] However, the COC macromolecular chain skeleton is mainly composed of carbon and hydrogen elements, with a low limiting oxygen index (LOI). It releases a large amount of heat and smoke during the combustion process, which greatly limits the application and promotion of COC materials. Summary of the invention

[0004] In view of the above defects, the present invention provides a flame-retardant cycloolefin copolymer composite material, wherein the composite material is a porous molecular sieve (such as ZSM-5 molecular sieve, etc.) or a porous molecular sieve modified by boric acid, etc. as a flame retardant synergist, and is added to a COC matrix together with an intumescent flame retardant to form a COC flame-retardant composite material. The limiting oxygen index (LOI) of the obtained COC composite material can reach 28%, and the LOI is increased by 100% (the LOI of pure COC is 14%), and the peak heat release rate (pHRR) of the cone calorimetry test (CCT) is reduced by 75% to 368.45kW / m 2 (The pHRR of pure COC is 1368.72kW / m 2 ).

[0005] The technical solution of the present invention:

[0006] The first technical problem to be solved by the present invention is to provide a flame-retardant cycloolefin copolymer composite material, which includes raw materials in the following proportions: 70 to 80 parts by weight of cycloolefin copolymer, 20 to 30 parts by weight of flame retardant, and 0.1 to 5 parts by weight of flame retardant synergist; wherein the flame retardant synergist is a porous molecular sieve or a modified substance obtained by modifying a porous molecular sieve with boric acid.

[0007] Furthermore, the porous molecular sieve is a molecular sieve capable of catalyzing esterification reaction, including: ZSM-5 molecular sieve, mesoporous SiO2 or MCM-41 molecular sieve, etc.

[0008] Furthermore, the cycloolefin copolymer can be selected from brand 8007 produced by TOPAS Corporation of the United States, or other brands, such as 9003, 5013, 6013, 6017, etc.

[0009] Furthermore, the flame retardant is an intumescent flame retardant.

[0010] Preferably, the flame retardant is an intumescent flame retardant obtained by mixing APP (ammonium polyphosphate) and PER (pentaerythritol) in a ratio of 3:1.

[0011] Furthermore, when the flame retardant synergist is a modified substance obtained by modifying a porous molecular sieve with boric acid, the amount of boric acid added accounts for 5% to 50% of the total mass of the boric acid and the porous molecular sieve.

[0012] Preferably, the amount of boric acid added is 20% to 30% of the total mass of the boric acid and the porous molecular sieve.

[0013] Furthermore, when the flame retardant synergist is a modified substance obtained by modifying a porous molecular sieve with boric acid, the flame retardant synergist is prepared by the following method: first, the porous molecular sieve is added to deionized water, boric acid is added after ultrasonic mixing, and ultrasonic treatment is continued for 20 to 40 minutes (preferably 30 minutes); then the flame retardant synergist is obtained by centrifugation and drying; wherein the amount of boric acid added accounts for 5% to 50% of the total mass of the boric acid and the porous molecular sieve.

[0014] Furthermore, in the preparation method of the flame retardant synergist, the ultrasonic treatment time is 20 to 40 minutes, preferably 30 minutes.

[0015] Furthermore, in the method for preparing the flame retardant synergist, the solid-liquid mass ratio of the porous molecular sieve to deionized water is 1:5-10.

[0016] Furthermore, in the method for preparing the flame retardant synergist, the drying temperature is 90° C. to 110° C., and the drying time is 12 hours to 24 hours.

[0017] The second technical problem to be solved by the present invention is to provide a method for preparing the flame-retardant cycloolefin copolymer composite material. The preparation method comprises: preparing the composite material by melt blending the raw materials.

[0018] Furthermore, the preparation method comprises: premixing the raw materials, then melting and extruding them in a twin-screw extruder, and finally injection molding.

[0019] The third technical problem to be solved by the present invention is to point out that a porous molecular sieve or a porous molecular sieve modified with boric acid can be used as a flame retardant synergist, wherein the porous molecular sieve is a ZSM-5 molecular sieve, a mesoporous SiO2 or a MCM-41 molecular sieve.

[0020] Furthermore, the flame retardant synergist is a modified substance obtained by modifying the porous molecular sieve with boric acid, and the amount of boric acid added accounts for 5% to 50% of the total mass of the boric acid and the porous molecular sieve; preferably 20% to 30%.

[0021] In the present invention, the flame retardant synergist refers to a synergist that can synergistically flame retard the material after being added together with the flame retardant.

[0022] Furthermore, the porous molecular sieve or the porous molecular sieve modified with boric acid is used as a flame retardant synergist of the cycloolefin copolymer, and synergistically flame retards the cycloolefin copolymer together with the intumescent flame retardant.

[0023] Beneficial effects of the present invention:

[0024] The porous molecular sieve or the porous molecular sieve modified by boric acid of the present invention is used as a flame retardant synergist and is added to a COC matrix together with an intumescent flame retardant to form a COC flame retardant composite material. The limiting oxygen index (LOI) of the obtained COC composite material can reach 28%, the LOI is increased by 100% (the LOI of pure COC is 14%), and the peak heat release rate (pHRR) of the cone calorimetry test (CCT) is reduced by 75% to 368.45kW / m 2 (The pHRR of pure COC is 1368.72kW / m 2 ). Description of the drawings:

[0025] Figure 1 This is a SEM micrograph of the modified ZSM-5 molecular sieve (25BZ5) prepared in Example 5 of the present invention.

[0026] Figure 2 The XPS test spectra (a) and the B1s fine spectra (b) of the modified ZSM-5 molecular sieves 5BZ5, 10BZ5, 15BZ5, 20BZ5 ​​and 25BZ5 prepared in Examples 1 to 5 of the present invention are shown in FIG. Figure 2 (b) It can be clearly seen in the fine spectrum that the appearance of the B1s peak at 193.4 eV indicates that the boric acid is successfully loaded, and the peak area gradually increases with the increase in the amount of boric acid added. XPS quantitative analysis shows that the loading amounts of boric acid are 2.17%, 7.48%, 7.11%, 8.95%, and 9.23%, respectively.

[0027] Figure 3 is the infrared spectra of the modified ZSM-5 molecular sieves 5BZ5, 10BZ5, 15BZ5, 20BZ5 ​​and 25BZ5 prepared in Examples 1 to 5 of the present invention; Figure 3 It can be seen that the wave number is 1393cm -1 The strong absorption peak indicates the formation of BO bond, and as the amount of boric acid added increases, the absorption peak gradually strengthens, indicating that the B loading amount gradually increases.

[0028] Figure 4 is a SEM micrograph of the COC flame retardant composite material prepared in Example 5 of the present invention, after CCT testing, in which 25BZ5 was added; Figure 4It can be seen that BZ5 molecular sieve cooperates with IFR to form a smooth and dense carbon layer during the flame retardant process, and improving the oxygen isolation protection ability is beneficial to improving the flame retardant performance. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be described in detail and completely below. However, the embodiments of the present invention are not limited thereto. Based on the embodiments of the present invention, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention.

[0030] Example 1

[0031] S1: First, add 15 g of ZSM-5 to 100 mL of deionized water, stir evenly, and then put it into an ultrasonic instrument with a power of 300 W. After ultrasonication for 10 min, add 0.789 g of H3BO3 and ultrasonicate for another 30 min. After the end, centrifuge and dry at 110 ° C overnight to obtain a modified ZSM-5 molecular sieve sample (referred to as 5BZ5);

[0032] S2: American Topas COC 8007S-04 cycloolefin copolymer (COC8007 for short) was dried in a vacuum oven at 60°C for 12 hours, and APP (ammonium polyphosphate), PER (pentaerythritol) and 5BZ5 were dried in a vacuum oven at 80°C for 12 hours and weighed. The weight ratios were as follows: COC8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1) and 5BZ5 was 1wt%;

[0033] S3: pre-mixing the raw materials; then adding the mixed materials into a twin-screw extruder, and extruding the mixed materials at a screw speed of 30 r / min and a melt temperature of 200° C. for injection molding;

[0034] S4: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC1.

[0035] Example 2

[0036] S1: First, add 15 g of ZSM-5 to 100 mL of deionized water, stir evenly, and then put it into an ultrasonic instrument with a power of 300 W. After ultrasonication for 10 min, add 1.667 g of H3BO3 and ultrasonicate for another 30 min. After the end, centrifuge and dry at 110 ° C overnight to obtain a modified ZSM-5 molecular sieve sample (denoted as 10BZ5);

[0037] S2: 8007, APP, PER and 10BZ5 were dried in a vacuum drying oven at 60°C and 80°C for 12 hours and then weighed. The weight ratios were as follows: 8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1) and 10BZ5 was 1wt%;

[0038] S3: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200° C. for injection molding;

[0039] S4: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC2.

[0040] Embodiment 3:

[0041] S1: First, add 15 g of ZSM-5 to 100 mL of deionized water, stir evenly, and then put it into an ultrasonic instrument with a power of 300 W. After ultrasonication for 10 min, add 2.647 g of H3BO3 and ultrasonicate for another 30 min. After the end, centrifuge and dry at 110 ° C overnight to obtain a modified ZSM-5 molecular sieve sample (denoted as 15BZ5);

[0042] S2: 8007, APP, PER and 15BZ5 were dried in a vacuum oven at 60°C and 80°C for 12 hours and then weighed. The weight ratios were as follows: 8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1) and 15BZ5 was 1wt%;

[0043] S3: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200° C. for injection molding;

[0044] S4: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC3.

[0045] Example 4

[0046] S1: First, add 15 g of ZSM-5 to 100 mL of deionized water, stir evenly, and then put it into an ultrasonic instrument with a power of 300 W. After ultrasonication for 10 min, add 3.750 g of H3BO3 and ultrasonicate for another 30 min. After the end, centrifuge and dry at 110 ° C overnight to obtain a modified ZSM-5 molecular sieve sample (denoted as 20BZ5);

[0047] S2: 8007, APP, PER and 20BZ5 ​​were dried in a vacuum drying oven at 60°C and 80°C for 12 hours and then weighed. The weight ratios were as follows: 8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1) and 20BZ5 ​​was 1wt%;

[0048] S3: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200° C. for injection molding;

[0049] S4: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC4.

[0050] Example 5

[0051] S1: First, add 15 g of ZSM-5 to 100 mL of deionized water, stir evenly, and then put it into an ultrasonic instrument with a power of 300 W. After ultrasonication for 10 min, add 5.000 g of H3BO3 and ultrasonicate for another 30 min. After the end, centrifuge and dry at 110 ° C overnight to obtain a modified ZSM-5 molecular sieve sample (denoted as 25BZ5);

[0052] S2: 8007, APP, PER and 25BZ5 were dried in a vacuum drying oven at 60°C and 80°C for 12 hours and then weighed. The weight ratios were as follows: 8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1) and 25BZ5 was 1wt%;

[0053] S3: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200° C. for injection molding;

[0054] S4: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC5.

[0055] Example 6

[0056] S1: First, add 15 g of ZSM-5 to 100 mL of deionized water, stir evenly, and then put it into an ultrasonic instrument with a power of 300 W. After ultrasonication for 10 min, add 6.428 g of H3BO3 and ultrasonicate for another 30 min. After the end, centrifuge and dry at 110 ° C overnight to obtain a modified ZSM-5 molecular sieve sample (referred to as 30BZ5);

[0057] S2: 8007, APP, PER and 15BZ5 were dried in a vacuum drying oven at 60°C and 80°C for 12 hours and then weighed. The weight ratios were as follows: 8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1) and 30BZ5 was 1wt%;

[0058] S3: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200° C. for injection molding;

[0059] S4: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC6.

[0060] Example 7

[0061] S1: First, add 15 g of ZSM-5 to 100 mL of deionized water, stir evenly, and then put it into an ultrasonic instrument with a power of 300 W. After ultrasonication for 10 min, add 10.00 g of H3BO3 and ultrasonicate for another 30 min. After the end, centrifuge and dry at 110 ° C overnight to obtain a modified ZSM-5 molecular sieve sample (denoted as 40BZ5);

[0062] S2: 8007, APP, PER and 15BZ5 were dried in a vacuum drying oven at 60°C and 80°C for 12 hours and then weighed. The weight ratios were as follows: 8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1) and 40BZ5 was 1wt%;

[0063] S3: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200° C. for injection molding;

[0064] S4: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC7.

[0065] Example 8

[0066] S1: First, add 15 g of ZSM-5 to 100 mL of deionized water, stir evenly, and then put it into an ultrasonic instrument with a power of 300 W. After ultrasonication for 10 min, add 15 g of H3BO3 and ultrasonicate for another 30 min. After the end, centrifuge and dry at 110 ° C overnight to obtain a modified ZSM-5 molecular sieve sample (referred to as 50BZ5);

[0067] S2: 8007, APP, PER and 15BZ5 were dried in a vacuum oven at 60°C and 80°C for 12 hours and then weighed. The weight ratios were as follows: 8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1) and 50BZ5 was 1wt%;

[0068] S3: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200° C. for injection molding;

[0069] S4: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC8.

[0070] Example 9

[0071] S1: 8007, APP, PER and unmodified ZSM-5 molecular sieve were dried in a vacuum drying oven at 60°C and 80°C for 12 hours and then weighed. The weight ratios were as follows: 8007 was 75wt%, IFR was 24wt%, (APP:PER=3:1), and ZSM-5 molecular sieve was 1wt%;

[0072] S2: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200°C for injection molding;

[0073] S3: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC8.

[0074] Comparative Example 1

[0075] S1: Weigh 8007 after drying it in a vacuum drying oven at 60°C for 12 hours;

[0076] S2: Add 8007 into a twin-screw extruder, melt-extrude the mixture at a screw speed of 30 r / min and a melt temperature of 200°C, and perform injection molding;

[0077] S3: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC-D1.

[0078] Comparative Example 2

[0079] S1: 8007, APP and PER were dried in a vacuum drying oven at 60°C and 80°C for 12 hours and then weighed. The weight ratio was as follows: 8007 was 75wt%, IFR was 25wt%, (APP:PER = 3:1);

[0080] S2: adding the mixed material into a twin-screw extruder, and extruding the mixed material at a screw speed of 30 r / min and a melt temperature of 200°C for injection molding;

[0081] S3: The extruded material is pelletized, dried, and hot-pressed. The composite material sample is recorded as COC-D2.

[0082] LOI refers to the minimum oxygen concentration required for a material to burn in a mixed flow of oxygen and nitrogen under specific conditions, which is used to judge the difficulty of a material to burn in the air. The higher the oxygen index of a material, the less likely it is to burn. Generally, LOI < 22% is flammable, LOI between 22-27% is combustible, and LOI > 27% is difficult to burn.

[0083] CCT can simulate the burning conditions of materials in real fires and is a crucial test method for evaluating the combustion performance of materials. The heat released during the combustion process is calculated based on the oxygen consumption of the material during combustion. It also includes some other detailed data, mainly the total heat release rate (THR), pHRR, char yield and other important parameters.

[0084] The limiting oxygen index test is carried out in accordance with the plastic oxygen index method ASTM D2863-97, and the sample size is 130mm×6.5mm×3mm. The cone calorimetry test is carried out in accordance with the international standard ISO 5660, and the thermal radiation power is set to 35kW / m 2 , the sheet size is 100mm×100mm×3mm.

[0085] Table 1 Raw material ratios of Examples 1-9 of the present invention and Comparative Examples

[0086]

[0087] Table 2 Flame retardant properties of COC composites

[0088]

[0089] “ / ” means there is no test result yet.

Claims

1. A flame retardant cycloolefin copolymer composite material, characterized in that: The composite material comprises raw materials in the following proportions: 70-80 parts by weight of cycloolefin copolymer, 20-30 parts by weight of flame retardant, and 0.1-5 parts by weight of flame retardant synergist; wherein the flame retardant synergist is a porous molecular sieve or a modified substance obtained by modifying the porous molecular sieve with boric acid.

2. The flame-retardant cycloolefin copolymer composite material according to claim 1, characterized in that: The porous molecular sieve includes: ZSM-5 molecular sieve, mesoporous SiO2 or MCM-41 molecular sieve.

3. A flame retardant cycloolefin copolymer composite material according to claim 1 or 2, characterized in that: The flame retardant is an intumescent flame retardant; Preferably, the flame retardant is an intumescent flame retardant obtained by mixing ammonium polyphosphate and pentaerythritol in a ratio of 3:

1.

4. The flame retardant cycloolefin copolymer composite material according to any one of claims 1 to 3, characterized in that: The flame retardant synergist is a modified substance obtained by modifying a porous molecular sieve with boric acid, and the amount of boric acid added accounts for 5% to 50% of the total mass of the boric acid and the porous molecular sieve; Preferably, the amount of boric acid added is 20% to 30% of the total mass of the boric acid and the porous molecular sieve.

5. The flame retardant cycloolefin copolymer composite material according to any one of claims 1 to 4, characterized in that: The flame retardant synergist is a modified substance obtained by modifying a porous molecular sieve with boric acid. The modified substance is prepared by the following method: firstly, the porous molecular sieve is added to deionized water, and boric acid is added after ultrasonic mixing, and ultrasonic treatment is continued; then, the modified substance is obtained by centrifugation and drying.

6. The flame-retardant cycloolefin copolymer composite material according to claim 5, characterized in that: The ultrasonic treatment time is 20 to 40 minutes; Furthermore, the solid-liquid mass ratio of the porous molecular sieve to deionized water is 1:5-10; Furthermore, the drying temperature is 90° C. to 110° C., and the drying time is 12 hours to 24 hours.

7. The method for preparing the flame-retardant cycloolefin copolymer composite material according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: melt-blending various raw materials to obtain the composite material.

8. A porous molecular sieve or a porous molecular sieve modified with boric acid is used as a flame retardant synergist, wherein: The porous molecular sieve is ZSM-5 molecular sieve, mesoporous SiO2 or MCM-41 molecular sieve.

9. The porous molecular sieve or the porous molecular sieve modified with boric acid according to claim 8 is used as a flame retardant synergist, characterized in that: In the porous molecular sieve modified with boric acid, the amount of boric acid added accounts for 5% to 50% of the total mass of the boric acid and the porous molecular sieve; preferably 20% to 30%.

10. The porous molecular sieve or the porous molecular sieve modified with boric acid according to claim 8 or 9 is used as a flame retardant synergist, characterized in that: The porous molecular sieve or the porous molecular sieve modified with boric acid is used as a flame retardant synergist for cycloolefin copolymer.