GTRB polymer composite sole material and manufacturing method of customized sole
Through GTRB polymer composite sole material and customized sole production method, the problem of difficulty in recycling existing rubber soles is solved, and the mechanical performance and recyclability of the sole are improved, meeting order requirements and reducing resource waste.
Patent Information
- Application Number
- CN202411194398.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
Existing rubber sole materials are difficult to recycle, resulting in environmental pollution and waste of resources.
Using GTRB polymer composite sole materials, including SBS thermoplastic elastomer, EVA particles, TR thermoplastic elastomer, cycloane oil, natural rubber, butyl rubber, styrene butyl rubber, silica and expansion agent, through customized sole production methods, Ensure the mechanical properties and recyclability of the sole.
It achieves the mechanical performance improvement and recyclability of the sole, complies with GRS standards, improves the apparent and intrinsic performance pass rate of customized sole, meets order requirements and reduces resource waste.
Abstract
Description
Technical Field
[0001] The invention relates to a sole material, in particular to a polymer composite sole material and a method for making a customized sole. Background Art
[0002] GTRB is a globally recyclable polymer composite thermoplastic rubber developed with SBS thermoplastic elastomer as base material and GRS (full name in English: Global Recycled Standard, referred to as GRS, Chinese: Global Recycling Standard) as standard. In GTRB, G stands for GRS, T stands for TR thermoplastic elastomer, and RB stands for rubber (rubber in English: Rubber). It has excellent mechanical properties and wear resistance. Compared with existing rubber soles, it has better elasticity, is not easy to deform, and is more wear-resistant. As daily necessities and decorative items, the amount of shoes used and eliminated is quite amazing. After the existing rubber soles are eliminated, their soles cannot be recycled as renewable resources, nor can they be biodegraded, so that the soles of discarded shoes will cause serious pollution and harm to the environment.
[0003] Therefore, there is an urgent need for a new sole material with better mechanical properties and recyclability. Summary of the invention
[0004] The purpose of the present invention is to provide a GTRB polymer composite sole material. The sole made of the GTRB polymer composite sole material has good mechanical properties and can be recycled as a renewable resource.
[0005] Another object of the present invention is to provide a method for making a customized sole, wherein the sole made by the method has good mechanical properties and can be recycled as a renewable resource.
[0006] To achieve the above object, the present invention provides a GTRB polymer composite sole material, which comprises, by weight:
[0007] 40-50 parts of SBS thermoplastic elastomer;
[0008] 10-15 parts of EVA particles;
[0009] 5-10 parts TR thermoplastic elastomer;
[0010] 5-10 parts of naphthenic oil;
[0011] 4-6 parts of natural rubber;
[0012] 2-3 parts of butadiene rubber;
[0013] 1-2 parts of styrene-butadiene rubber;
[0014] 1-2 parts of silicon dioxide;
[0015] 0.5-2.0 parts of expansion agent.
[0016] Preferably, in the GTRB polymer composite sole material of the present invention, the EVA particles are EVA particles of model 7350M produced by Formosa Plastics Corporation in Taiwan, China.
[0017] Preferably, in the GTRB polymer composite sole material of the present invention, the expansion agent is azodicarbonamide or dimethylterephthalamide.
[0018] The method for making a customized sole provided by the present invention comprises the following steps:
[0019] Step (1): Collect data; collect foot data according to the order;
[0020] Step (2): Modeling: performing three-dimensional modeling using three-dimensional design software according to the foot data to form a three-dimensional model of the sole;
[0021] Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model;
[0022] Step (4): drying treatment; putting the GTRB polymer composite sole material according to any one of claims 1 to 3 into a drying device for drying treatment to obtain a sole raw material;
[0023] Step (5): trial production of samples; taking appropriate sole raw materials and putting them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; and recording parameters during the injection molding process, wherein the parameters include temperature parameters and pressure parameters of the injection molding;
[0024] Step (6): testing the sample; performing a wear resistance test, a bending test and an anti-slip test on the sole sample;
[0025] Step (7): test comparison; compare the test result of the sole sample with the sole requirement data in the order; if it meets the sole requirement data in the order, proceed to step (8); if it does not meet the sole requirement data in the order, repeat the above steps (5) to (6) until it meets the sole requirement data in the order; wherein each time step (5) is repeated, at least one of the temperature parameter and the pressure parameter of the injection molding is different from the previous one;
[0026] Step (8): Batch production: all the sole raw materials are placed in a stirring device and stirred evenly to obtain a production mixture. According to the parameters of the injection molding process recorded in step (5), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.
[0027] By adopting the above technical scheme, the beneficial effects of the present invention are as follows: the present invention adopts SBS thermoplastic elastomer and EVA particles as the main principles; TR thermoplastic elastomer is added to increase the lightness, softness, elasticity and wear resistance of the manufactured sole; naphthenic oil is added to further increase the softness and elasticity of the manufactured sole; by adding and matching natural rubber, butadiene rubber, styrene butadiene rubber, silica and expansion agent, the molecular structure of the entire material is changed to achieve improvement in lightness, softness, elasticity, wear resistance and anti-slip property; the polymer composite material prepared by the above formula of the present invention is particularly suitable for making soles, has a light specific gravity and can be recycled as a renewable resource, and meets the GRS standard. The present invention adopts the above formula as raw material to carry out the method for making customized soles, so that the made customized soles are not only light in specific gravity and can be recycled as renewable resources, but also have excellent softness, elasticity, wear resistance and anti-slip properties. At the same time, the method for making customized soles of the present invention directly collects foot data from the order given by the customer, and uses the foot data to perform three-dimensional modeling of the sole and make a mold, so that the customized soles made by mold injection molding are consistent with the specifications, sizes, styles and appearances required by the customer order, which greatly improves the qualified rate of the appearance of the customized soles. At the same time, in the production process, by verifying the qualification of the trial production samples, the optimal parameters of the injection molding machine for injection molding the customized soles are confirmed, which greatly improves the qualified rate of the intrinsic performance of the customized soles. It can be seen that the production method of the present invention independently performs dual optimization and improvement from two aspects of the appearance and intrinsic performance of the soles, so that the customized soles produced according to the production method of the present invention can not only highly meet the requirements of the order and recyclability, but also have excellent softness, elasticity, wear resistance and anti-slip properties of the soles. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present application are clearly and completely described below in conjunction with specific implementation examples, and the technical solutions of the present invention are explained. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0029] The GTRB polymer composite sole material of the present invention comprises, by weight: 40-50 parts of SBS thermoplastic elastomer; 10-15 parts of EVA particles; 5-10 parts of TR thermoplastic elastomer; 5-10 parts of naphthenic oil; 4-6 parts of natural rubber; 2-3 parts of butadiene rubber; 1-2 parts of styrene-butadiene rubber; 1-2 parts of silicon dioxide; and 0.5-2.0 parts of swelling agent. Preferably, in order to further improve the lightness, softness, elasticity, wear resistance and anti-slip properties of the sole made of the GTRB polymer composite sole material of the present invention, and at the same time ensure the recyclability of the GTRB polymer composite sole material of the present invention and the sole made therefrom, the EVA particles of the present invention are EVA particles of model 7350M produced by Formosa Plastics Corporation in Taiwan, China. Furthermore, the expansion agent of the present invention is preferably azodicarbonamide or dimethylterephthalamide; using azodicarbonamide or dimethylterephthalamide as the expansion agent can better exert its expansion effect in combination with other raw materials, thereby improving the lightness, softness and elasticity of the manufactured sole.
[0030] The method for making a customized sole provided by the present invention comprises the following steps:
[0031] Step (1): Collect data; collect foot data according to the order.
[0032] Step (2): Modeling: Performing three-dimensional modeling using three-dimensional design software based on the foot data to form a three-dimensional model of the sole.
[0033] Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model.
[0034] Step (4): drying treatment; 40-50 parts by weight of SBS thermoplastic elastomer, 10-15 parts of EVA particles, 5-10 parts of TR thermoplastic elastomer, 5-10 parts of cyclohexane oil, 4-6 parts of natural rubber, 2-3 parts of butadiene rubber, 1-2 parts of styrene-butadiene rubber, 1-2 parts of silicon dioxide, and 0.5-2.0 parts of swelling agent are respectively put into a drying device for drying treatment to obtain a sole raw material; specifically, the amount of the sole raw material used can be determined by those skilled in the art according to the number of customized soles to be produced without any creative labor, and will not be repeated again.
[0035] Step (5): trial production of samples; taking appropriate sole raw materials and placing them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; at the same time, recording parameters during the injection molding process, the parameters including the temperature parameters and pressure parameters of the injection molding; specifically, the temperature parameters of the injection molding are 130-145°C, and the pressure parameters of the injection molding are 30-45MPa.
[0036] Step (6): testing samples; performing abrasion resistance test, bending test and anti-slip test on the sole samples.
[0037] Step (7): test comparison; compare the test results of the sole sample with the sole requirement data in the order; if it meets the sole requirement data in the order, proceed to step (8); if it does not meet the sole requirement data in the order, repeat the above steps (5) to (6) until it meets the sole requirement data in the order; wherein each time step (5) is repeated, at least one of the temperature parameters and pressure parameters of the injection molding is different from the previous one.
[0038] Step (8): Batch production: all the sole raw materials are placed in a stirring device and stirred evenly to obtain a production mixture. According to the parameters of the injection molding process recorded in step (5), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.
[0039] Specifically, the 3D design software used in the present invention can be existing design software such as Creo, Catia, UG, Solidworks, etc. Those skilled in the art can make a choice according to actual needs without any creative labor, and will not be described in detail here.
[0040] By adopting the above technical scheme, the present invention adopts SBS thermoplastic elastomer and EVA particles as the main principles; TR thermoplastic elastomer is added to increase the lightness, softness, elasticity and wear resistance of the manufactured sole; naphthenic oil is added to further increase the softness and elasticity of the manufactured sole; by adding and matching natural rubber, butadiene rubber, styrene butadiene rubber, silica and expansion agent, the molecular structure of the whole material is changed to achieve the improvement of lightness, softness, elasticity, wear resistance and anti-slip property; the polymer composite material prepared by the above formula of the present invention is particularly suitable for making soles, has a light specific gravity and can be recycled as a renewable resource, and meets the GRS standard. The present invention adopts the above formula as raw material to carry out the method for making customized soles, so that the made customized soles are not only light in specific gravity and can be recycled as renewable resources, but also have excellent softness, elasticity, wear resistance and anti-slip properties. At the same time, the method for making customized soles of the present invention directly collects foot data from the order given by the customer, and uses the foot data to perform three-dimensional modeling of the sole and make a mold, so that the customized soles made by mold injection molding are consistent with the specifications, sizes, styles and appearances required by the customer order, which greatly improves the qualified rate of the appearance of the customized soles. At the same time, in the production process, by verifying the qualification of the trial production samples, the optimal parameters of the injection molding machine for injection molding the customized soles are confirmed, which greatly improves the qualified rate of the intrinsic performance of the customized soles. It can be seen that the production method of the present invention independently performs dual optimization and improvement from two aspects of the appearance and intrinsic performance of the soles, so that the customized soles produced according to the production method of the present invention can not only highly meet the requirements of the order and recyclability, but also have excellent softness, elasticity, wear resistance and anti-slip properties of the soles.
[0041] Embodiment 1, the method for making a customized sole provided by the present invention comprises the following steps:
[0042] Step (1): Collect data; collect foot data according to the order; specifically, the order requires that the wear resistance of the customized sole be DIN <100, the bending of the customized sole be >50,000 times; and the friction coefficient of the customized sole be ≥0.3.
[0043] Step (2): Modeling: Performing three-dimensional modeling using three-dimensional design software based on the foot data to form a three-dimensional model of the sole.
[0044] Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model.
[0045] Step (4): Drying treatment: 40 parts by weight of SBS thermoplastic elastomer, 10 parts of EVA particles, 5 parts of TR thermoplastic elastomer, 5 parts of cyclohexane oil, 4 parts of natural rubber, 2 parts of butadiene rubber, 1 part of styrene-butadiene rubber, 1 part of silicon dioxide, and 0.5 parts of swelling agent are respectively put into a drying equipment for drying treatment to obtain a sole raw material.
[0046] Step (5): trial production of samples; taking appropriate sole raw materials and placing them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; at the same time, recording parameters during the injection molding process, the parameters including the temperature parameters and pressure parameters of the injection molding; specifically, the temperature parameters of the injection molding are 130-135°C, and the pressure parameters of the injection molding are 30-35MPa.
[0047] Step (6): testing samples; performing wear resistance test, bending test and anti-slip test on the sole samples; the test results are: sole wear resistance DIN = 95, customized sole bending = 62,000 times; customized sole friction coefficient in dry environment = 0.42; customized sole friction coefficient in wet environment = 0.35.
[0048] Step (7): test and compare; compare the test results of the sole sample with the sole requirement data in the order; and confirm that the sole requirement data in the order is met;
[0049] Step (8): Batch production: Put all the sole raw materials into a stirring device and stir them evenly to obtain a production mixture. According to the parameters in the injection molding process recorded in step (5) (i.e., the temperature parameter of injection molding is 130-145°C, and the pressure parameter of injection molding is 30-45MPa), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.
[0050] Embodiment 2, the method for making a customized sole provided by the present invention comprises the following steps:
[0051] Step (1): Collect data; collect foot data according to the order; specifically, the order requires that the wear resistance of the customized sole be DIN <100, the bending of the customized sole be >50,000 times; and the friction coefficient of the customized sole be ≥0.3.
[0052] Step (2): Modeling: Performing three-dimensional modeling using three-dimensional design software based on the foot data to form a three-dimensional model of the sole.
[0053] Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model.
[0054] Step (4): Drying treatment: 50 parts of SBS thermoplastic elastomer, 15 parts of EVA particles, 10 parts of TR thermoplastic elastomer, 10 parts of cyclohexane oil, 6 parts of natural rubber, 3 parts of butadiene rubber, 2 parts of styrene-butadiene rubber, 2 parts of silicon dioxide, and 2.0 parts of swelling agent, measured by weight, are respectively put into a drying equipment for drying treatment to obtain a sole raw material.
[0055] Step (5): trial production of samples; taking appropriate sole raw materials and placing them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; at the same time, recording parameters during the injection molding process, the parameters including the temperature parameters and pressure parameters of the injection molding; specifically, the temperature parameters of the injection molding are 120-130°C, and the pressure parameters of the injection molding are 35-40MPa.
[0056] Step (6): testing samples; performing wear resistance test, bending test and anti-slip test on the sole samples; the test results are: sole wear resistance DIN = 90, customized sole bending = 45,000 times; customized sole friction coefficient in dry environment = 0.32; customized sole friction coefficient in wet environment = 0.28.
[0057] Step (7): test comparison; compare the test results of the sole sample with the sole requirement data in the order; if it does not meet the sole requirement data in the order, it is necessary to change the injection molding parameters and re-execute steps (5) and (6) until it meets the sole requirement data in the order; after changing the parameters and re-executing steps (5) and (6) three times, the test sample obtained for the fourth time meets the sole requirement data in the order, and the temperature parameters of the fourth injection molding are 135-140°C, and the pressure parameters of the injection molding are 33-38MPa.
[0058] Step (8): Batch production: Put all the sole raw materials into a stirring device and stir them evenly to obtain a production mixture. According to the parameters in the injection molding process recorded in step (5) (i.e., the temperature parameter of injection molding is 135-140°C, and the pressure parameter of injection molding is 33-38MPa), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.
[0059] Embodiment 3, the method for making a customized sole provided by the present invention comprises the following steps:
[0060] Step (1): Collect data; collect foot data according to the order; specifically, the order requires that the wear resistance of the customized sole be DIN <100, the bending of the customized sole be >50,000 times; and the friction coefficient of the customized sole be ≥0.3.
[0061] Step (2): Modeling: Performing three-dimensional modeling using three-dimensional design software based on the foot data to form a three-dimensional model of the sole.
[0062] Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model.
[0063] Step (4): Drying treatment: 45 parts of SBS thermoplastic elastomer, 12.5 parts of EVA particles, 7.5 parts of TR thermoplastic elastomer, 7.5 parts of cyclohexane oil, 5 parts of natural rubber, 2.5 parts of butadiene rubber, 1.5 parts of styrene-butadiene rubber, 1.5 parts of silicon dioxide, and 1.25 parts of swelling agent, measured by weight, are respectively put into a drying equipment for drying treatment to obtain a sole raw material.
[0064] Step (5): trial production of samples; taking appropriate sole raw materials and placing them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; at the same time, recording parameters during the injection molding process, the parameters including the temperature parameters and pressure parameters of the injection molding; specifically, the temperature parameters of the injection molding are 135-140°C, and the pressure parameters of the injection molding are 35-40MPa.
[0065] Step (6): testing samples; performing wear resistance test, bending test and anti-slip test on the sole samples; the test results are: sole wear resistance DIN = 97, customized sole bending = 63,000 times; customized sole friction coefficient in dry environment = 0.45; customized sole friction coefficient in wet environment = 0.37.
[0066] Step (7): Test and compare; compare the test results of the sole sample with the sole requirement data in the order; and ensure that the sole requirement data in the order is met.
[0067] Step (8): Batch production: Put all the sole raw materials into a stirring device and stir them evenly to obtain a production mixture. According to the parameters in the injection molding process recorded in step (5) (i.e., the temperature parameter of injection molding is 135-140°C, and the pressure parameter of injection molding is 35-40MPa), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.
[0068] Embodiment 4, the method for making a customized sole provided by the present invention comprises the following steps:
[0069] Step (1): Collect data; collect foot data according to the order; specifically, the order requires that the wear resistance of the customized sole be DIN <100, the bending of the customized sole be >50,000 times; and the friction coefficient of the customized sole be ≥0.3.
[0070] Step (2): Modeling: Performing three-dimensional modeling using three-dimensional design software based on the foot data to form a three-dimensional model of the sole.
[0071] Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model.
[0072] Step (4): Drying treatment: 44 parts of SBS thermoplastic elastomer, 14 parts of EVA particles, 9 parts of TR thermoplastic elastomer, 7 parts of cyclohexane oil, 6 parts of natural rubber, 2 parts of butadiene rubber, 1 part of styrene-butadiene rubber, 1 part of silicon dioxide, and 1 part of swelling agent, measured by weight, are respectively put into a drying device for drying treatment to obtain a sole raw material.
[0073] Step (5): trial production of samples; taking appropriate sole raw materials and placing them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; at the same time, recording parameters during the injection molding process, the parameters including the temperature parameters and pressure parameters of the injection molding; specifically, the temperature parameters of the injection molding are 137-142°C, and the pressure parameters of the injection molding are 32-37MPa.
[0074] Step (6): testing samples; performing wear resistance test, bending test and anti-slip test on the sole samples; the test results are: sole wear resistance DIN = 95, customized sole bending = 71,000 times; customized sole friction coefficient in dry environment = 0.46; customized sole friction coefficient in wet environment = 0.41.
[0075] Step (7): Test and compare; compare the test results of the sole sample with the sole requirement data in the order; and ensure that the sole requirement data in the order is met.
[0076] Step (8): Batch production: Put all the sole raw materials into a stirring device and stir them evenly to obtain a production mixture. According to the parameters in the injection molding process recorded in step (5) (i.e., the temperature parameter of injection molding is 137-142°C, and the pressure parameter of injection molding is 32-37MPa), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.
[0077] Embodiment 5, the method for making a customized sole provided by the present invention comprises the following steps:
[0078] Step (1): Collect data; collect foot data according to the order; specifically, the order requires that the wear resistance of the customized sole be DIN <100, the bending of the customized sole be >50,000 times; and the friction coefficient of the customized sole be ≥0.3.
[0079] Step (2): Modeling: Performing three-dimensional modeling using three-dimensional design software based on the foot data to form a three-dimensional model of the sole.
[0080] Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model.
[0081] Step (4): Drying treatment: 48 parts of SBS thermoplastic elastomer, 14 parts of EVA particles, 6 parts of TR thermoplastic elastomer, 7 parts of cyclohexane oil, 4 parts of natural rubber, 3 parts of butadiene rubber, 1.8 parts of styrene-butadiene rubber, 1.6 parts of silicon dioxide, and 2 parts of swelling agent, measured by weight, are respectively put into a drying equipment for drying treatment to obtain a sole raw material.
[0082] Step (5): trial production of samples; taking appropriate sole raw materials and placing them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; at the same time, recording parameters during the injection molding process, the parameters including the temperature parameters and pressure parameters of the injection molding; specifically, the temperature parameters of the injection molding are 140-145°C, and the pressure parameters of the injection molding are 40-45MPa.
[0083] Step (6): testing samples; performing wear resistance test, bending test and anti-slip test on the sole samples; the test results are: sole wear resistance DIN = 92, customized sole bending = 75,000 times; customized sole friction coefficient in dry environment = 0.41; customized sole friction coefficient in wet environment = 0.36.
[0084] Step (7): Test and compare; compare the test results of the sole sample with the sole requirement data in the order; and ensure that the sole requirement data in the order is met.
[0085] Step (8): Batch production: Put all the sole raw materials into a stirring device and stir them evenly to obtain a production mixture. According to the parameters in the injection molding process recorded in step (5) (i.e., the temperature parameter of injection molding is 140-145°C, and the pressure parameter of injection molding is 40-45MPa), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.
[0086] Embodiment 6, the method for making a customized sole provided by the present invention comprises the following steps:
[0087] Step (1): Collect data; collect foot data according to the order; specifically, the order requires that the wear resistance of the customized sole be DIN <100, the bending of the customized sole be >50,000 times; and the friction coefficient of the customized sole be ≥0.3.
[0088] Step (2): Modeling: Performing three-dimensional modeling using three-dimensional design software based on the foot data to form a three-dimensional model of the sole.
[0089] Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model.
[0090] Step (4): Drying treatment: 42 parts of SBS thermoplastic elastomer, 11 parts of EVA particles, 9 parts of TR thermoplastic elastomer, 8 parts of cyclohexane oil, 5.5 parts of natural rubber, 2.8 parts of butadiene rubber, 1 part of styrene-butadiene rubber, 1 part of silicon dioxide, and 1.8 parts of swelling agent, measured by weight, are respectively put into a drying equipment for drying treatment to obtain a sole raw material.
[0091] Step (5): trial production of samples; taking appropriate sole raw materials and placing them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; at the same time, recording parameters during the injection molding process, the parameters including the temperature parameters and pressure parameters of the injection molding; specifically, the temperature parameters of the injection molding are 138-143°C, and the pressure parameters of the injection molding are 39-44MPa.
[0092] Step (6): testing samples; performing wear resistance test, bending test and anti-slip test on the sole samples; the test results are: sole wear resistance DIN = 94, customized sole bending = 68,000 times; customized sole friction coefficient in dry environment = 0.42; customized sole friction coefficient in wet environment = 0.33.
[0093] Step (7): Test and compare; compare the test results of the sole sample with the sole requirement data in the order; and ensure that the sole requirement data in the order is met.
[0094] Step (8): Batch production: Put all the sole raw materials into a stirring device and stir them evenly to obtain a production mixture. According to the parameters in the injection molding process recorded in step (5) (i.e., the temperature parameter of injection molding is 138-143°C, and the pressure parameter of injection molding is 39-44MPa), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.
[0095] In the above-mentioned embodiments 1-6 of the present invention, the EVA particles are preferably EVA particles of model 7350M produced by Formosa Plastics Corporation in Taiwan, China; and the swelling agent is preferably azodicarbonamide or dimethylterephthalamide.
[0096] It can be seen from the above that the customized soles made using the GTRB polymer composite sole material and the customized sole manufacturing method of the present invention can not only highly meet the requirements of the order and recyclability, but also have excellent performance in sole softness, elasticity, wear resistance and anti-slip properties.
[0097] In addition, the injection molding technology and the testing method of the test sample involved in the present invention are well known to ordinary technicians in the field and will not be described in detail here.
[0098] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present invention is defined by the appended claims rather than the above description, so it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention. At the same time, what is disclosed above is only the preferred embodiment of the present invention, and of course it cannot be used to limit the scope of the rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention are still within the scope covered by the present invention.
Claims
1. A GTRB polymer composite sole material, characterized in that: The parts by weight include: 40-50 parts of SBS thermoplastic elastomer; 10-15 parts of EVA particles; 5-10 parts TR thermoplastic elastomer; 5-10 parts of naphthenic oil; 4-6 parts of natural rubber; 2-3 parts of butadiene rubber; 1-2 parts of styrene-butadiene rubber; 1-2 parts of silicon dioxide; 0.5-2.0 parts of expansion agent.
2. The GTRB polymer composite sole material according to claim 1, characterized in that: The EVA particles are EVA particles of model 7350M produced by Formosa Plastics Corporation in Taiwan, China.
3. The GTRB polymer composite sole material according to claim 1, characterized in that: The expansion agent is azodicarbonamide or dimethylterephthalamide.
4. A method for making a customized sole, characterized in that: The steps include: Step (1): Collect data; collect foot data according to the order; Step (2): Modeling: performing three-dimensional modeling using three-dimensional design software according to the foot data to form a three-dimensional model of the sole; Step (3): making a mold; using the three-dimensional design software to design a mold model that is consistent with the three-dimensional model of the sole, and making a mold that is consistent with the mold model; Step (4): drying treatment; putting the GTRB polymer composite sole material according to any one of claims 1 to 3 into a drying device for drying treatment to obtain a sole raw material; Step (5): trial production of samples; taking appropriate sole raw materials and putting them into a stirring device for uniform stirring to obtain a sample mixture, injecting the sample mixture into the mold cavity of the mold through an injection molding machine and cooling and molding to form a sole sample; and recording parameters during the injection molding process, wherein the parameters include temperature parameters and pressure parameters of the injection molding; Step (6): testing the sample; performing a wear resistance test, a bending test and an anti-slip test on the sole sample; Step (7): test comparison; compare the test result of the sole sample with the sole requirement data in the order; if it meets the sole requirement data in the order, proceed to step (8); if it does not meet the sole requirement data in the order, repeat the above steps (5) to (6) until it meets the sole requirement data in the order; Each time step (5) is repeated, at least one of the temperature parameter and the pressure parameter of the injection molding is different from the previous one; Step (8): Batch production: all the sole raw materials are placed in a stirring device and stirred evenly to obtain a production mixture. According to the parameters of the injection molding process recorded in step (5), the production mixture is injected into the mold cavity of the mold through an injection molding machine and cooled to form a customized sole.