Reversible thermochromic ABS (Acrylonitrile Butadiene Styrene) plastic and preparation method thereof
By adding temperature-sensitive colorant, lubricant, gloss enhancer, toughener and antioxidant to ABS plastic, the high-gloss reversible thermal discoloration ABS plastic is prepared by using the twin-screw extrusion mechanism to prepare high-gloss reversible thermal discoloration ABS plastic, the reversible thermal discoloration in the prior art is solved. Color-changing ABS composite materials are not suitable for injection molding production, and achieve high mechanical properties and reversible color changes of ABS plastics, and are suitable for injection molding production of children's toys.
Patent Information
- Application Number
- CN202410542175.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing reversible thermal discoloration ABS composite materials are mainly suitable for 3D printing technology and are not suitable for injection molding of toy products. It is difficult to achieve reversible thermal discoloration effect in injection molding of ABS plastics.
85-95% transparent grade ABS resin, 0.3-1% temperature-sensitive color change agent, 0.1-0.5% lubricant, 5-10% light enhancer, 0-10% toughener and 0.1-0.7% are used. The antioxidants are melted, extruded, granulated and dried by a twin-screw extruder to prepare high-gloss reversible thermochromic ABS plastic.
It realizes the high mechanical properties, simple injection molding and reversible color changes of ABS plastics, and is suitable for mass production of children's toys, increasing the attractiveness and fun of the products.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, in particular to a reversible thermochromic ABS plastic and a preparation method thereof. Background Art
[0002] ABS plastic is non-toxic and odorless. It is a ternary copolymer of acrylonitrile (A), butadiene (B), and styrene (S). The relative content of the three monomers can be changed arbitrarily to make various resins. ABS plastic has the common properties of the three components. A makes it resistant to chemical corrosion and heat, and has a certain surface hardness. B makes it highly elastic and tough. S makes it have the processing and molding characteristics of thermoplastics and improves electrical properties. By changing the proportion of the three components, the various properties of ABS can be changed, making it widely used in the fields of automobiles, textiles, instruments and meters, toy production, 3D printing, and construction. In addition, ABS resin can also be added with color powder or masterbatch to achieve product color and appearance diversity.
[0003] For example, the Chinese patent application with application publication number CN106905655A discloses a reversible thermochromic ABS composite material, a preparation method and its application in 3D printing. The ABS composite material is composed of 5-25 parts of masterbatch, 100 parts of ABS resin, 0.3-0.8 parts of dispersant 1 and 5-7 parts of inorganic filler; the masterbatch is composed of 50-70% ABS resin, 5-12% dispersant 2 and 20-40% colorant; the colorant is composed of more than one reversible thermochromic powder, or more than one reversible thermochromic powder and pigment. The ABS composite material of the invention is mainly used in 3D printing technology. The printed products undergo reversible thermochromic changes, which can achieve a variety of appearances. However, such composite materials are only suitable for 3D printing technology and are not suitable for injection molding production of toy products.
[0004] If we want to apply the reversible thermochromic technology to the injection molding of ABS plastic toy products, the existing technology needs to be improved. Summary of the invention
[0005] The purpose of the present invention is to provide a reversible thermochromic ABS plastic and a preparation method thereof. The reversible thermochromic ABS plastic is used in toy products produced by injection molding.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The reversible thermochromic ABS plastic of the present invention comprises the following components in terms of mass percentage:
[0008] ABS resin: 85-95%;
[0009] Thermochromic agent: 0.3-1%;
[0010] Lubricant: 0.1-0.5%;
[0011] Brightener: 5-10%;
[0012] Toughening agent: 0-10%;
[0013] Antioxidant: 0.1~0.7%.
[0014] According to the above solution, the ABS resin is a transparent ABS resin, and preferably has a light transmittance of more than 85%.
[0015] According to the above scheme, the thermochromic agent is a reversible thermochromic powder or a reversible thermochromic masterbatch. Preferably, the thermochromic agent is a reversible thermochromic powder or a reversible thermochromic masterbatch that changes from colored to colorless or from colored to colored, such as colored to colorless, such as bright red, pink, rose red, vermilion, orange, yellow, sky blue, aqua, turquoise, violet, dark blue, royal blue, grass green, green, black, etc.; colored to colored, such as green to yellow, purple to red, green to blue, purple to blue, blue to pink, blue to green, red to yellow, orange to yellow, black to red, black to yellow, etc.
[0016] According to the above scheme, the thermochromic agent uses a micron-level microcapsule color-changing agent that is resistant to high temperature and weathering, and can repeatedly change color as the temperature rises or falls. In addition, color-changing pigments of different colors, different temperatures, and different series can be matched and combined with each other to meet a variety of color change requirements.
[0017] According to the above scheme, the thermochromic temperature of the thermochromic agent is one of 5°C, 12°C, 15°C, 18°C, 22°C, 25°C, 28°C, 31°C, 33°C, 35°C, 38°C, 40°C, 45°C, and 65°C.
[0018] According to the above scheme, the lubricant is polytetrafluoroethylene modified polyethylene wax with a melting point of 126°C. Adding polytetrafluoroethylene modified polyethylene wax to ABS resin can achieve internal lubrication and demolding effects. At the same time, it can significantly reduce the friction coefficient of the surface of the plastic product and improve the wear resistance of the plastic product itself. It is suitable for the production of children's toys.
[0019] According to the above scheme, the brightener is one or both of talcum powder or muscovite powder. More specifically, the talcum powder or muscovite powder and the lubricant can synergistically impart high gloss to ABS plastic, thereby greatly improving the aesthetics of the product.
[0020] According to the above scheme, the toughening agent is one or more of SBS, SEBS, POE or high rubber powder, and the toughening agent plays a role in reducing the brittleness of ABS plastic and improving the toughness of ABS plastic. Among them, SBS, SEBS, POE or high rubber powder have good compatibility with ABS resin, and the effect of improving toughness is better, which is conducive to the manufacture of toys by injection molding of ABS plastic.
[0021] According to the above scheme, the antioxidant is a compound of phosphite antioxidant 168 and hindered phenol antioxidant 1010. Preferably, the antioxidant is a compound of phosphite antioxidant 168 and hindered phenol antioxidant 1010 in a mass ratio of 1:1. It should be noted that hindered phenol antioxidant 1010 is a primary antioxidant, which plays an antioxidant role for a long time by capturing free radicals generated during the degradation of plastics; phosphite antioxidant 168 is an auxiliary antioxidant, which achieves the purpose of antioxidant by decomposing the peroxides generated by further degradation of plastics. The joint use of primary antioxidant + auxiliary antioxidant can produce a synergistic effect and has good antioxidant performance.
[0022] A method for preparing reversible thermochromic ABS plastic comprises the following steps:
[0023] (1) Evenly mixing the dried thermochromic agent and talcum powder to obtain a color-changing powder;
[0024] (2) mixing the color-changing toner with the dried ABS resin, lubricant, toughening agent, and antioxidant at high speed;
[0025] (3) A twin-screw extruder is used to melt, extrude, granulate and dry the mixed raw materials to obtain high-gloss reversible thermochromic ABS plastic.
[0026] According to the above scheme, the processing parameters of the twin-screw extruder are: main engine speed: 400r / min, feed rate: 40kg / hour, and screw processing temperature is set to 210-230°C.
[0027] The beneficial effects of the present invention are:
[0028] The reversible thermochromic ABS plastic of the present invention has good mechanical properties and is simple to be injection molded, and can be used for mass production of children's toys. The product has high gloss and the color of the product has the function of reversible change, presenting different colors at different ambient temperatures, thereby increasing the attractiveness and interest of the toy product. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described below in conjunction with embodiments.
[0030] The ABS resin in the embodiment of the present invention is a high-transparent ABS resin purchased from Dongguan Heshengyuan New Material Technology Co., Ltd.; the thermochromic agent is the thermochromic microcapsule powder of Jinhua Lijin Technology Co., Ltd.; the toughening agent is SBS, i.e., styrene-butadiene-styrene block copolymer, and the selected model is SBS Maoming Petrochemical YH-796; the phosphite antioxidant 168 and the hindered phenol antioxidant 1010 are both purchased from BASF.
[0031] The present invention provides a high-gloss reversible thermochromic ABS plastic and a preparation method thereof, which comprises the following components in terms of mass percentage:
[0032] Transparent ABS resin, 85-95%, transmittance above 85%, melt flow rate 25g / 10min, tested according to ISO1133 standard;
[0033] Thermochromic agent, 0.3-1%, purple to red, purple to blue, blue to pink, orange to yellow, four types of color-changing agents, color-changing temperature 45°C;
[0034] Lubricant, 0.1-0.5%, polytetrafluoroethylene modified polyethylene wax, melting point 126°C;
[0035] Brightener, 5-10%, talcum powder, particle size 800-1000 mesh;
[0036] Toughener, 0-5%, styrene-butadiene-styrene block copolymer (SBS);
[0037] Antioxidant, 0.1-0.7%, phosphite antioxidant 168 and hindered phenol antioxidant 1010 are compounded in a mass ratio of 1:1;
[0038] The preparation steps of a reversible thermochromic ABS plastic of the present invention are as follows:
[0039] (1) Evenly mixing the dried thermochromic agent and talcum powder to obtain a color-changing powder;
[0040] (2) mixing the color-changing toner with the dried ABS plastic, lubricant, toughening agent, and antioxidant at high speed;
[0041] (2) A twin-screw extruder is used to melt, extrude, granulate and dry the mixed raw materials to obtain a high-gloss reversible thermochromic ABS plastic, wherein the processing parameters of the twin-screw extruder are: main engine speed: 400 r / min, feed rate: 40 kg / hour, and screw processing temperature is set to 210-230°C.
[0042] The following is a more specific example.
[0043] Table 1 Weight parts of raw material components of Examples 1-4 and Comparative Examples 1-2
[0044]
[0045] Performance evaluation method and implementation standards:
[0046] Test specimen preparation: The test specimen is molded by injection molding machine according to the standard specimen mold. Before preparing the specimen, the test material must be dried in an oven at 110±5℃ for 4 to 5 hours.
[0047] The test specimens must be placed in an environment of 23±2℃ and relative humidity of 50±5% for at least 24 hours and tested in an environment of 23±2℃ and relative humidity of 50±5%.
[0048] The tensile strength was tested according to ASTM D638, with a tensile rate of 50 mm / min and a gauge length of 50 cm;
[0049] Impact strength is tested according to ASTM D256 Izod notched impact test standard;
[0050] The specific gravity is tested according to GB / T1033 standard.
[0051] The color difference was tested using a XriteCi 7800 spectrophotometer, and the average value was read after 3 tests.
[0052] Table 2 Test results of Examples 1-4 and Comparative Example 2
[0053]
[0054]
[0055] It can be seen from the above test results that the ABS plastic of the present invention has an obvious reversible thermochromic effect, and the plastic has high tensile strength, high elongation at break, good toughness, and good mechanical properties, which meets the requirements of injection molding production of children's toys.
[0056] The above description is only a preferred embodiment of the present invention, so all equivalent changes or modifications made according to the structure, characteristics and principles described in the scope of the patent application of the present invention are included in the scope of the patent application of the present invention.
Claims
1. A reversible thermochromic ABS plastic, characterized in that: According to mass percentage, it contains the following components: ABS resin: 85-95%; Thermochromic agent: 0.3-1%; Lubricant: 0.1-0.5%; Brightener: 5-10%; Toughening agent: 0-10%; Antioxidant: 0.1~0.7%.
2. The reversibly thermochromic ABS plastic according to claim 1, characterized in that: The ABS resin is a transparent grade ABS resin.
3. The reversibly thermochromic ABS plastic according to claim 1, characterized in that: The thermochromic agent is a reversible thermochromic powder or a reversible thermochromic masterbatch.
4. The reversibly thermochromic ABS plastic according to claim 1, characterized in that: The lubricant is polytetrafluoroethylene modified polyethylene wax.
5. The reversibly thermochromic ABS plastic according to claim 1, characterized in that: The brightener is one or both of talc powder and muscovite powder.
6. The reversibly thermochromic ABS plastic according to claim 1, characterized in that: The toughening agent is one or more of SBS, SEBS, POE or high-rubber powder.
7. The reversibly thermochromic ABS plastic according to claim 1, characterized in that: The antioxidant is prepared by compounding a phosphite antioxidant 168 and a hindered phenol antioxidant 1010.
8. The reversibly thermochromic ABS plastic according to claim 7, characterized in that: The antioxidant is prepared by compounding a phosphite antioxidant 168 and a hindered phenol antioxidant 1010 in a mass ratio of 1:
1.
9. The method for preparing the reversibly thermochromic ABS plastic according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Evenly mixing the dried thermochromic agent and talcum powder to obtain a color-changing powder; (2) mixing the color-changing toner with the dried ABS resin, lubricant, toughening agent, and antioxidant at high speed; (3) A twin-screw extruder is used to melt, extrude, granulate and dry the mixed raw materials to obtain high-gloss reversible thermochromic ABS plastic.
10. The method for preparing reversibly thermochromic ABS plastic according to claim 9, characterized in that: The processing parameters of the twin-screw extruder are: main engine speed: 400r / min, feed rate: 40kg / hour, and screw processing temperature is set at 210-230°C.