Method for synergistically enhancing wear resistance of resin-based composite material for traction machine through zinc oxide and silicon carbide
By synergistically adding zinc oxide and silicon carbide to the resin-based composite material, combined with dry mixing and hot press sintering technology, the wear resistance and friction coefficient stability of the resin-based friction materials for traction machines are solved, and the material is high resistance to the material Abrasive and stable friction performance, suitable for friction materials for elevator traction machines.
Patent Information
- Application Number
- CN202411025439.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing resin-based friction materials are difficult to meet the requirements of high wear resistance and friction coefficient stability of the traction machine. It is difficult to meet the mechanical and friction performance requirements of the material when silicon carbide or zinc oxide are added separately.
By synergistically adding zinc oxide and silicon carbide of specific shapes, sizes and contents to the resin-based composite, combined with the dry mixing and hot press sintering process, the mechanical and friction wear properties of the material are adjusted.
The high wear resistance and stable friction coefficient of resin-based composite materials are achieved, the compression strength and average friction coefficient of the material are improved, and the volume wear rate is reduced, meeting the needs of the traction machine.
Smart Images

Figure CN118931103A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resin-based friction materials, in particular to a method for enhancing the wear resistance of a resin-based composite material for a traction machine. Background Art
[0002] Friction material is a key material used in various vehicles and power machinery, relying on friction to absorb or transmit power, thereby performing braking or transmission functions; its mechanical properties determine whether it can withstand the forces during processing and use, and friction and wear performance directly determines the safety and stability during service. Therefore, the composition of friction materials must be precisely controlled to achieve the regulation of their performance. At the same time, for friction materials used in traction machines, the average friction coefficient should be maintained between 0.30 and 0.60, so that the traction machine has good service stability; but with the development of modern industry, higher requirements are placed on its service life.
[0003] Resin-based composite materials have been widely used in various fields due to their advantages such as low density, strong composition design and easy forming. Among them, resin-based friction materials, as one of the main friction materials today, are usually composed of binders, reinforcing fibers, lubricating phases, friction enhancers and fillers. The weight and content of the binder can be changed to adjust the mechanical properties of the composite material, and the ratio and content of the lubricating phase and the friction enhancer can be adjusted to achieve the regulation of its tribological properties. Zinc oxide and silicon carbide are commonly used friction performance regulators, which often have the functions of adjusting the mechanical strength, high temperature resistance, oxidation resistance, friction coefficient, friction coefficient stability and wear resistance of the material. Their shape, particle size and content need to be precisely controlled. Studies have shown that when silicon carbide and zinc oxide are added alone to enhance the phase, it is difficult to meet the requirements of the friction coefficient of the traction machine; the composite addition of reinforced ortho-cresol new epoxy resin has low overall material strength due to insufficient resin strength. At the same time, the Chinese patent "Anti-skid and wear-resistant load-carrying vehicle tire rubber and preparation method" with publication number CN 107163309A discloses an anti-skid and wear-resistant load-carrying vehicle tire rubber and preparation method. By adding graphene oxide, nano-titanium dioxide, nano-silicon carbide, carbon black, zinc oxide, tackifier, antioxidant, vulcanizer and accelerator, etc., the rubber material obtained by mixing, extruding and granulating has good anti-skid and wear-resistant properties, and has good use value in load-carrying vehicles. However, its disadvantage is that it does not list specific values such as average friction coefficient and volume wear rate for reference. Therefore, it is urgent to develop a resin-based composite material for traction machines with a stable friction coefficient (0.30-0.60) and high wear resistance. Summary of the invention
[0004] The purpose of the present invention is to improve the mechanical and friction and wear properties of resin-based composite materials by adding friction performance modifiers zinc oxide and silicon carbide, and to provide a method for synergistically enhancing the wear resistance of resin-based composite materials for traction machines by zinc oxide and silicon carbide.
[0005] In order to achieve the above object, the present invention provides the following scheme:
[0006] The present invention provides a method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide. The preparation method comprises the following steps:
[0007] (1) Weigh powders in order according to the mass fractions of 0% to 30% binder, 0% to 40% reinforcing fiber, 0% to 20% friction reducer, 0% to 20% zinc oxide, 0% to 20% silicon carbide, and 0% to 60% filler;
[0008] (2) The raw materials are then placed in a ball mill for dry mixing, and dried after the dry mixing is completed;
[0009] (3) placing the dried material into a pretreated mold for hot pressing and sintering, keeping the temperature, and then cooling it to room temperature in the furnace to obtain the resin-based composite material.
[0010] Furthermore, the binder in step (1) is cashew nut shell oil modified phenolic resin, and the average diameter of the binder is 16.81 μm. The function of the binder is to bond the components into a whole.
[0011] Furthermore, the reinforcing fibers in step (1) are short basalt fibers, the average length of the reinforcing fibers is 164.75 μm, and the average diameter is 6.77 μm. The reinforcing fibers serve as a skeleton to bear the load during processing and use.
[0012] Furthermore, the friction reducer in step (1) is artificial graphite, and the average particle size of the friction reducer is 273.25 μm. The function of the friction reducer is to reduce noise.
[0013] Furthermore, the zinc oxide in step (1) is short columnar, micron-sized particles with an average particle size of 0.35 μm. The function of the zinc oxide is to increase the average friction coefficient. Figure 1 and Figure 2 They are the microscopic morphology and particle size distribution of zinc oxide used in this article.
[0014] Furthermore, the silicon carbide in step (1) is blade-shaped, micron-sized particles with an average particle size of 31.97 μm. The function of the silicon carbide is to improve mechanical strength and wear resistance. Figure 3 and Figure 4 They are the microscopic morphology and particle size distribution of silicon carbide used in this article.
[0015] Furthermore, the filler in step (1) is barium sulfate, and the average particle size of the filler is 12.81 μm. The function of the filler is to fill space.
[0016] Furthermore, step (2) is dry-mixed in a vertical planetary ball mill.
[0017] Furthermore, in step (2), the raw materials except the reinforcing fiber are dry-mixed in a vertical planetary ball mill at a speed of 150 r / min for 15 hours, and then the reinforcing fiber is added and dry-mixed at a speed of 150 r / min for 3 hours.
[0018] Furthermore, the drying in step (2) is carried out in an electric heated air drying oven.
[0019] Furthermore, step (2) is dried at 60° C. for 2 h.
[0020] Furthermore, the pre-treated mold in step (3) is a mold that has been cleaned with alcohol and has a layer of 0.01 mm thick graphite release paper padded on the upper and lower surfaces.
[0021] Furthermore, during the hot pressing sintering in step (3), the temperature is raised from room temperature to 175° C. at a heating rate of 10° C. / min at 15 MPa, kept at that temperature for 60 minutes, and then cooled to room temperature in the furnace.
[0022] The invention provides a method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide.
[0023] The present invention also provides the use of the resin-based composite material in friction materials for traction machines, and the average friction coefficient of the composite material should be controlled within the range of 0.30 to 0.60.
[0024] The present invention discloses the following technical effects:
[0025] The present invention improves the mechanical and friction and wear properties of resin-based composite materials by simultaneously adding zinc oxide and silicon carbide of specific shapes, sizes and contents. Among them, zinc oxide is mainly used to improve the friction coefficient, and silicon carbide is used to improve the mechanical strength and wear resistance. The two synergistically improve the mechanical and friction and wear properties of resin-based composite materials. Compared with the related research on adding silicon carbide or zinc oxide resin-based composite materials alone, the organizational morphology is obviously different, and the compression strength, average friction coefficient and volume wear rate are all in a good range. At the same time, the two raw materials of zinc oxide and silicon carbide are low-cost and easy to obtain, and have good application value in the field of friction materials for elevator traction machines. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0027] Figure 1 The microscopic morphology of zinc oxide used in the present invention;
[0028] Figure 2 is a particle size distribution diagram of zinc oxide used in the present invention;
[0029] Figure 3 The microscopic morphology of silicon carbide used in the present invention;
[0030] Figure 4 is a particle size distribution diagram of silicon carbide used in the present invention;
[0031] Figure 5 This is a sintering process curve diagram of Example 4 of the present invention;
[0032] Figure 6 This is an infrared spectrum of the mixed powder of Example 4 of the present invention before and after sintering;
[0033] Figure 7 This is a microstructure morphology diagram of the resin-based composite material prepared in Example 4 of the present invention;
[0034] Figure 8 This is a microscopic morphology of the resin-based composite material prepared in Example 4 of the present invention after wear;
[0035] Fig. 9 Friction coefficient curves of the resin-based composite materials prepared in Examples 1 and 4 of the present invention;
[0036] Fig.10 Graph showing the average friction coefficient and volume wear rate of the resin-based composite materials prepared in Examples 1 and 4 of the present invention. DETAILED DESCRIPTION
[0037] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0038] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the stated range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0039] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art to which the invention belongs. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation and testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0040] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention without departing from the scope or spirit of the present invention.The present invention description and examples are intended to be exemplary only.
[0041] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended words, meaning including but not limited to.
[0042] Example 1
[0043] (1) Weigh 3.00 g of cashew nut shell oil-modified phenolic resin powder, 3.75 g of chopped basalt fiber, 0.30 g of artificial graphite, 0.00 g of zinc oxide powder, 0.00 g of silicon carbide powder, and 7.95 g of barium sulfate (mass fractions were 20%, 25%, 2%, 0%, 0%, and 53%, respectively), pour the raw materials except the fiber into a mixing tank, and then put it into an XQM-2 vertical planetary ball mill and dry mix it at a speed of 150 r / min for 15 h, then pour the chopped basalt fiber into it and dry mix it at a speed of 150 r / min for 3 h, and then pour the powder into a beaker and place it in a 101-2A electric heating blast drying oven and dry it at 60°C for 2 h.
[0044] (2) Clean the mold with alcohol and place a layer of graphite release paper (0.1 mm thick) on the upper and lower surfaces of the mold. Slowly pour the powder in step (1) into the mold and flatten it. Then, hot press sinter it in a HTEYP-30 flat plate vulcanizer to obtain a 20×20×5 mm 3The sample was sintered at 15 MPa at a rate of 10°C / min from room temperature to 175°C, kept at that temperature for 60 minutes, and then cooled to room temperature in the furnace. Thus, a resin-based composite material was obtained, and the material prepared in this embodiment was recorded as sample M0.
[0045] Take the M0 sample and use the HRA-50 Rockwell hardness tester to test the hardness of the composite material. The hardness test points of each sample are 5 points evenly distributed on the surface of the sample, and the average value is taken as the hardness of the sample. The compression test is carried out on the WDW-100C electronic universal testing machine. The sample size is 10×10×5mm 3 The loading rate is 0.01 mm / s. The compressive strength of the material is obtained by collecting the stress-strain values during the compression process. Each sample is measured three times, and the average value is taken as the final compressive strength of the sample.
[0046] Take the M0 sample and test its friction and wear performance on the CFT-I friction and wear testing machine. The sample size is 20×20×5mm. 3 The counter is an AISI-1045 steel ball with a diameter of 6 mm and a Rockwell hardness of 25 HRC. Before the test, the sample and the counter are polished with sandpaper and cleaned with alcohol to improve the reliability of the data obtained during the test. The test is carried out under dry friction conditions, with a test load of 20N, a reciprocating number of 500t / min, a reciprocating length of 5mm, and a reciprocating time of 30min.
[0047] Example 2
[0048] 3.00 g of cashew nut shell oil modified phenolic resin powder, 3.75 g of chopped basalt fiber, 0.30 g of artificial graphite, 1.35 g of zinc oxide powder, 0.00 g of silicon carbide powder, and 6.60 g of barium sulfate (mass fractions of 20%, 25%, 2%, 9%, 0%, and 44%, respectively) were weighed respectively. The mixing, drying, preparation process, and characterization methods were the same as those in Example 1. The material prepared in this example was recorded as sample M1.
[0049] Example 3
[0050] 3.00 g of cashew nut shell oil modified phenolic resin powder, 3.75 g of chopped basalt fiber, 0.30 g of artificial graphite, 1.35 g of zinc oxide powder, 0.30 g of silicon carbide powder, and 6.30 g of barium sulfate (mass fractions of 20%, 25%, 2%, 9%, 2%, and 42%, respectively) were weighed respectively. The mixing, drying, preparation process, and characterization methods were the same as those in Example 1. The material prepared in this example was recorded as sample M2.
[0051] Example 4
[0052] 3.00 g of cashew nut shell oil modified phenolic resin powder, 3.75 g of chopped basalt fiber, 0.30 g of artificial graphite, 1.35 g of zinc oxide powder, 0.75 g of silicon carbide powder, and 5.85 g of barium sulfate (mass fractions of 20%, 25%, 2%, 9%, 0%, and 39%, respectively) were weighed respectively. The mixing, drying, preparation process, and characterization methods were the same as those in Example 1. The material prepared in this example was recorded as sample M3.
[0053] The sintering process curve of this embodiment is shown in Figure 5 The infrared spectra of the mixed powder of this embodiment before and after sintering are shown in Figure 6 The surface morphology of the resin-based composite material prepared in this embodiment is shown in Figure 7 The microstructure of the resin-based composite material prepared in this embodiment after wear is shown in Figure 8 .
[0054] Example 5
[0055] 3.00 g of cashew nut shell oil-modified phenolic resin powder, 3.75 g of chopped basalt fiber, 0.30 g of artificial graphite, 1.35 g of zinc oxide powder, 1.20 g of silicon carbide powder, and 5.40 g of barium sulfate (mass fractions of 20%, 25%, 2%, 9%, 8%, and 36%, respectively) were weighed respectively. The mixing, drying, preparation process, and characterization methods were the same as those in Example 1. The material prepared in this example was recorded as sample M4.
[0056] Performance Characterization Results
[0057] The friction curves of the resin-based composite materials prepared in Example 1 and Example 4 are shown in Fig. 9 The average friction coefficient and volume wear rate of the resin-based composite materials prepared in Example 1 and Example 4 are shown in Fig.10 . Table 1 shows the physical and mechanical properties test results of the resin-based composite materials M0-M4 samples obtained in Examples 1-5, and Table 2 shows the friction and wear properties test results of the resin-based composite materials M0-M4 samples obtained in Examples 1-5. It can be seen from the test results that the resin-based composite materials prepared by adding zinc oxide and silicon carbide in the present invention have good mechanical properties and can withstand the forces during processing and use. It was also found that zinc oxide can effectively increase the average friction coefficient of the composite material, silicon carbide can effectively increase the hardness and compression strength of the composite material and reduce the volume wear rate. At the same time, the addition of zinc oxide and silicon carbide can make the composite material maintain a high friction coefficient while having an extremely low volume wear rate, and have both safety and durability.
[0058] Table 1 Physical and mechanical properties of composite materials
[0059]
[0060] Table 2 Average friction coefficient, variance and volume wear rate of composite materials
[0061]
[0062] It can be seen from the above embodiments that the present invention greatly improves the mechanical and friction and wear properties of the cashew nut shell oil-modified phenolic resin-based composite material by adding silicon carbide and zinc oxide of specific shape, size and content, has higher safety and longer service life, and has good application value.
[0063] The cashew nut shell oil-modified phenolic resin-based composite material prepared by adding silicon carbide and zinc oxide of specific shape, size and content has unique organizational morphology, high compression strength, average friction coefficient and extremely low volume wear rate, and has good application value in the field of friction materials for elevator traction machines.
[0064] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide, characterized in that: The preparation comprises the following steps: (1) weighing powders in order according to mass fractions of 0% to 30% binder, 0% to 40% reinforcing fiber, 0% to 20% friction reducer, 0% to 20% zinc oxide, 0% to 20% silicon carbide, and 0% to 60% filler; (2) then placing the raw materials in a ball mill for dry mixing, and drying after the dry mixing is completed; (3) placing the dried powder in a pretreated mold for hot pressing and sintering, keeping the temperature, and then cooling to room temperature with the furnace to obtain the resin-based composite material.
2. The method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide according to claim 1, characterized in that: The adhesive in step (1) is cashew nut shell oil-modified phenolic resin, and the average particle size of the adhesive is 16.81 μm.
3. The method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide according to claim 1, characterized in that: The reinforcing fibers in step (1) are chopped basalt fibers, and the average length of the reinforcing fibers is 164.75 μm and the average diameter is 6.77 μm.
4. The method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide according to claim 1, characterized in that: The friction reducer in step (1) is artificial graphite, and the average particle size of the friction reducer is 273.25 μm.
5. The method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide according to claim 1, characterized in that: The zinc oxide in step (1) is short columnar, micron-sized particles with an average particle size of 0.35 μm.
6. The method of claim 1 for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide, characterized in that: The silicon carbide in step (1) is blade-shaped, micron-sized particles with an average particle size of 31.97 μm.
7. The method of claim 1 for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide, characterized in that: The filler in step (1) is barium sulfate, and the average particle size of the filler is 12.81 μm.
8. The method of claim 1 for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide, characterized in that: Step (2) dry mixing in a vertical planetary ball mill.
9. The method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide according to claim 1, characterized in that: Step (2) In a vertical planetary ball mill, the raw materials except the reinforcing fiber are dry-mixed at a speed of 150 r / min for 15 hours, and then the reinforcing fiber is added and dry-mixed at a speed of 150 r / min for 3 hours.
10. The method of claim 1 for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide, characterized in that: The drying in step (2) is carried out in an electric heated air drying oven at 60° C. for 2 h.
11. The method for synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide according to claim 1, characterized in that: Step (3) is sintered at 15 MPa and 175°C.
12. A resin-based composite material obtained by the method of synergistically enhancing the wear resistance of a resin-based composite material for a traction machine by using zinc oxide and silicon carbide as claimed in any one of claims 1 to 11.