Medium-strength carbon fiber composite material and preparation method thereof

Through the combination of T1100 grade carbon fiber and GME223 resin and hot melting process, the problem of insufficient bonding ability between high-strength medium-mode carbon fiber and resin is solved, the mechanical properties of the composite material are improved, and the high strength and lightweight requirements in the aerospace field are met.

CN118931108APending Publication Date: 2024-11-12CHENGDU AIRCRAFT INDUSTRY GROUP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411133559.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The lack of interface bonding ability between high-strength medium-mode carbon fiber and resin leads to composite layering and quality problems, which is difficult to meet the demand for lightweight, high-strength and high-stiff materials in the aerospace field.

Method used

T1100 grade carbon fiber and GME223 resin were used as a combination of materials, and medium-strength carbon fiber composite materials were prepared by hot melt coating and hot melt dipping method, optimizing the resin formula and process parameters, and improving the interlayer shear strength and mechanical properties.

Benefits of technology

It significantly improves the tensile and compressive strength and modulus of composite materials, enhances interlayer bonding performance, and meets the high strength, high stiffness and lightweight needs in the aerospace field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931108A_ABST
    Figure CN118931108A_ABST
Patent Text Reader

Abstract

The invention discloses a medium-strength carbon fiber composite material and a preparation method thereof, relates to the technical field of composite materials, and solves the technical problem that a carbon fiber composite material prepared in the prior art is difficult to meet application requirements. The medium-strength carbon fiber composite material is prepared by taking T1100-grade carbon fiber T1100-12K as a reinforcing material and GME223 resin as a matrix material, wherein the T1100-grade carbon fiber T1100-12K is used as the reinforcing material, and the GME223 resin is used as the matrix material; the average value of the interlaminar shear strength of the carbon fiber composite material is 98 MPa, and the minimum value is 87 MPa; the average value of the tensile strength of the carbon fiber composite material is 3003 MPa, and the minimum value of the tensile strength is 2734 MPa; the average value of the tensile modulus of the carbon fiber composite material is 217 GPa, and the minimum value of the tensile modulus of the carbon fiber composite material is 206 GPa; the average value of the compression strength of the carbon fiber composite material is 1437 MPa, and the minimum value of the compression strength of the carbon fiber composite material is 1328 MPa; the average value of the compression modulus of the carbon fiber composite material is 189 GPa, and the minimum value of the compression modulus of the carbon fiber composite material is 184 GPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite materials, and in particular to a medium-strength carbon fiber composite material and a preparation method thereof. Background Art

[0002] The composite material made of T1100 fiber-reinforced prepreg has a tensile strength of ≥2500MPa and a tensile modulus of ≥170GPa. The tensile and compressive strength of the composite material is about 20% higher than that of the T700 series composite materials, and the tensile modulus and compression modulus are about 30% higher. Therefore, the main load-bearing components such as the middle and front fuselage frames and beams of aviation models and the secondary load-bearing components such as skins and reinforced wall panels have an urgent need for domestically produced T1100 fiber-reinforced prepreg as the main material.

[0003] However, the high-strength medium modulus carbon fiber has a high surface inertness and a large difference in strength modulus with the resin, resulting in a lower interfacial bonding ability with the resin. If the epoxy resin and carbon fiber do not match, the composite material will be delaminated. At the same time, if the surface of the T1100-grade prepreg is uneven or the curing is uneven, it will cause a series of quality problems such as high porosity, poor glue, and rich glue in the composite parts, reducing the mechanical properties of the structure. Therefore, it is urgent to carry out technical research on composite material manufacturing. Summary of the invention

[0004] The present application provides a high-strength medium-mode prepreg and a preparation method and application thereof, which at least solves the technical problem that the carbon fiber composite materials prepared by the prior art are difficult to meet application requirements.

[0005] In order to solve the above technical problems, the embodiment of the present application provides: a medium-strength carbon fiber composite material, wherein the medium-strength carbon fiber composite material is prepared by using T1100-12K grade carbon fiber as a reinforcing material and GME223 resin as a matrix material;

[0006] The average interlaminar shear strength of the carbon fiber composite material is 98 MPa, and the minimum is 87 MPa;

[0007] The average tensile strength of the carbon fiber composite material is 3003 MPa, and the minimum is 2734 MPa;

[0008] The average tensile modulus of the carbon fiber composite material is 217 GPa, and the minimum is 206 GPa;

[0009] The average compressive strength of the carbon fiber composite material is 1437 MPa, and the minimum is 1328 MPa;

[0010] The average compression modulus of the carbon fiber composite material is 189 GPa, and the minimum is 184 GPa.

[0011] As some optional embodiments of the present application, the GME223 resin includes: an epoxy A component with an epoxy value between 0.88-0.91, an epoxy B component with an epoxy value between 0.49-0.51, an epoxy C component, an epoxy D component and an epoxy E component.

[0012] The epoxy C component is bisphenol A type epoxy resin; the epoxy D component is phenolphthalein based polyetherketone toughening agent; and the epoxy E component is 3,3'-diaminodiphenyl sulfone.

[0013] As some optional embodiments of the present application, the epoxy component A is a trifunctional m-aminophenol triglycidyl epoxy resin.

[0014] As some optional embodiments of the present application, the epoxy B component is a trifunctional o-cresol glycidyl ether type epoxy resin.

[0015] As some optional embodiments of the present application, the medium-strength carbon fiber composite material has a fiber surface density setting range of 132±4 g / ㎡ and a resin content of 33±3%; and is prepared by hot melt coating and hot melt dipping methods.

[0016] As some optional embodiments of the present application, the T1100-12K fiber density is 1.76 g / cm 3 , linear density 0.414g / m, tensile strength 7020MPa, tensile modulus 315GPa, and elongation at break 2.23%.

[0017] On the other hand, the embodiment of the present application further provides: a method for preparing the medium-strength carbon fiber composite material as described above, comprising the following steps:

[0018] After T1100-12K T1100 carbon fiber and GME223 resin are treated by hot melt coating and hot melt dipping; the assembled sealing bag after prepreg stacking is leak-checked, and then a vacuum pressure of ≤-0.90Bar is applied; the tank temperature is set to rise at a rate of 2℃ / min to 135±2℃; while heating, the pressure is set to 6.5±0.2Bar for 10 minutes; when the leading thermocouple reaches 130℃, the timing is started to keep the temperature constant for 90±5min; after the constant temperature is ended, the tank temperature is set to rise at a rate of 2℃ / min to 181±2℃; when the lagging thermocouple is heated to 177℃, the timing is started to keep the temperature constant for 180min±5min; the cooling rate is set to be ≤1.5℃ / min, and when the slowest thermocouple temperature drops to 60℃, the pressure and vacuum are released and the tank is taken out.

[0019] As some optional embodiments of the present application, the hot melt glue coating method includes the following steps:

[0020] The resin matrix is ​​placed on a heat-conductive belt to soften the resin matrix into a resin melt; the resin melt is introduced into the glue groove between the glue coating roller and the metering roller through the heat-conductive belt, and the resin melt is evenly coated on the release paper through a glue coating process, and the accuracy of the glue coating amount is controlled by a β instrument. After passing the test, the resin is rolled up for standby use.

[0021] As some optional embodiments of the present application, the gluing process includes: a maximum gluing speed of 2 m / min, a gap between the gluing / metering rollers of 0.10 to 0.12 mm, a setting temperature of the gluing roller of 70°C, a setting temperature of the melting plate of 80°C, a setting temperature of the cooling roller of 16°C, and a setting weight of the gluing machine of 32.5 g / m 2 .

[0022] As some optional embodiments of the present application, the hot melt dipping method includes the following steps:

[0023] Set the temperature of heating zone 1 to 65°C, heating zone 2 to 80°C, heating zone 2 to 75°C, cooling zone 2 to 16°C, the gap between the rollers to 0.35-0.40mm, and the dipping speed to 1-2g / m 2 , the T1100 grade reinforced carbon fiber is spread.

[0024] As some optional embodiments of the present application, the GME223 resin is prepared by the following steps:

[0025] Add 60 to 80 parts of epoxy component A, 20 to 30 parts of epoxy component B, and 4 to 8 parts of epoxy component C into a reaction kettle and mix them evenly at 90°C; then add 4 to 6 parts of epoxy component D and stir at 90°C for 15 to 30 minutes to mix evenly;

[0026] After heating to 135°C, stir and heat for 50 to 80 minutes to mix evenly; cool to 90°C, add 32 to 35 parts of epoxy E component, and stir for 10 to 30 minutes;

[0027] The mixture was cooled to 75° C., 1 to 3 parts of epoxy E component were added, and the mixture was stirred for 15 to 30 minutes to be uniformly mixed; after cooling to room temperature, GME223 resin was obtained.

[0028] Compared with the prior art, the medium-strength carbon fiber composite material provided in the present application is prepared by using T1100-grade carbon fiber T1100-12K as a reinforcing material and GME223 resin as a matrix material; the average interlaminar shear strength of the carbon fiber composite material is 98MPa, and the minimum is 87MPa; the average tensile strength of the carbon fiber composite material is 3003MPa, and the minimum is 2734MPa; the average tensile modulus of the carbon fiber composite material is 217GPa, and the minimum is 206GPa; the average compressive strength of the carbon fiber composite material is 1437MPa, and the minimum is 1328MPa; the average compression modulus of the carbon fiber composite material is 189GPa, and the minimum is 184GPa. The tensile and compressive strength of the composite material described in the present application is increased by about 20% compared with the T700-grade series composite material, and the tensile modulus and compression modulus are increased by about 30%, thereby better meeting the requirements of lightweight, high strength and high stiffness of aircraft structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the specific implementation of the present application or the technical solution in the prior art, the following is a brief introduction to the drawings required for the specific implementation or the prior art description. In all drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, each element or part is not necessarily drawn according to the actual scale.

[0030] Figure 1 It is the viscosity-temperature curve diagram of the GME223 resin involved in this application;

[0031] Figure 2 This is a DSC analysis chart of the curing time of the GME223 resin involved in this application;

[0032] Figure 3 This is a diagram of the prepreg curing molding process parameters involved in this application.

[0033] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0035] As mentioned above, the surface inertness of high-strength medium modulus carbon fiber is high, and the strength modulus between it and the resin is quite different, resulting in lower interfacial bonding ability with the resin. If the epoxy resin and carbon fiber do not match, the composite material will be delaminated. At the same time, if the surface of the T1100-grade prepreg is uneven or the curing is uneven, it will cause a series of quality problems such as high porosity, poor glue, and rich glue in the composite parts, reducing the mechanical properties of the structure. Therefore, it is urgent to carry out technical research on the design and manufacture of epoxy resin formulas suitable for high-strength medium modulus carbon fiber, high-strength medium modulus epoxy prepreg and composite material manufacturing.

[0036] That is, the modern aerospace industry pursues lightweight, high-strength and high-rigidity structural materials to improve aircraft performance and fuel efficiency. The introduction of high-strength medium-modulus carbon fiber, such as Torayca T1100G, has significantly improved the strength and stiffness of composite materials, making them an ideal choice for the aviation field. This material is not only widely used in the structure of commercial aircraft (such as B777, B787, A350, etc.), but also plays a key role in the design of military aircraft (such as F-22, F-35, B-2 and other stealth fighters) and helicopters (such as CH-53K).

[0037] Although high-strength medium modulus carbon fiber has excellent mechanical properties, the insufficient interfacial bonding ability between it and epoxy resin is an important challenge. This mismatch may lead to delamination of the composite material, thereby reducing the mechanical properties and durability of the structure. To solve this problem, it is necessary to carry out research on epoxy resin formulation design and manufacturing technology for high-strength medium modulus carbon fiber. The research focuses on improving the bonding strength between resin and fiber, optimizing the curing process to reduce porosity, and ensuring the quality and performance stability of the composite material.

[0038] Toray's leading position in the field of high-strength medium-modulus carbon fiber cannot be ignored. Its developed grades such as T1100G have been widely used in the global aerospace and high-end industrial markets, providing reliable material support for the lightweight structure of modern aircraft and spacecraft. However, the urgent need of domestic aviation equipment manufacturers for independent research and development of high-performance composite materials is also promoting the development and maturity of related domestic technologies.

[0039] With the continuous progress of the aerospace industry and the emergence of new technologies, it is expected that more composite materials and new resin systems based on high-strength medium-modulus carbon fibers will be introduced in the future. These new materials will further optimize the performance of composite materials, reduce production costs, and have higher sustainability and environmental friendliness to cope with the improvement of material performance and quality requirements for future aircraft and spacecraft.

[0040] In summary, high-strength medium-modulus carbon fiber and its matching with epoxy resin are important topics of concern in the aerospace field. Solving these technical challenges will promote the widespread application and further development of composite material technology in aviation equipment.

[0041] Based on this, an embodiment of the present application provides a medium-strength carbon fiber composite material, which is prepared by using T1100-grade carbon fiber T1100-12K as a reinforcing material and GME223 resin as a matrix material;

[0042] The average interlaminar shear strength of the carbon fiber composite material is 98 MPa, and the minimum is 87 MPa;

[0043] The average tensile strength of the carbon fiber composite material is 3003 MPa, and the minimum is 2734 MPa;

[0044] The average tensile modulus of the carbon fiber composite material is 217 GPa, and the minimum is 206 GPa;

[0045] The average compressive strength of the carbon fiber composite material is 1437 MPa, and the minimum is 1328 MPa;

[0046] The average compression modulus of the carbon fiber composite material is 189 GPa, and the minimum is 184 GPa.

[0047] It can be seen that the medium-strength carbon fiber composite material described in this application has several significant advantages compared to existing composite materials:

[0048] Superior strength and modulus: The composite material has an average tensile strength of 3003MPa and an average tensile modulus of 217GPa, indicating that it has very high strength and stiffness under tensile loading. This allows it to withstand greater loads and challenging working conditions in aerospace applications while maintaining a lightweight design of the structure.

[0049] Good interlaminar shear strength: The average interlaminar shear strength is 98MPa, which reflects its good bonding performance between composite layers, helps to reduce interlaminar shear cracking and failure of composite interface, and improves the durability and reliability of the overall structure.

[0050] Excellent compression performance: The average compression strength is 1437MPa and the average compression modulus is 189GPa, which shows the stability and strength of the material under compressive loading. This is especially important for aviation devices that need to work in complex stress environments.

[0051] Advanced Material Combination: Using a combination of T1100-12K carbon fiber and GME223 resin as the matrix material, combined with high-performance carbon fiber and an optimized resin system, helps improve the preparation process and final performance of the composite material, making it suitable for a wider range of applications.

[0052] That is, this medium-strength carbon fiber composite material not only excels in strength, stiffness and durability, but also improves the performance and reliability of the overall structure through optimized interlayer bonding and material formula design, making it a favorable choice in the modern aerospace field.

[0053] Specifically, the GME223 resin includes: an epoxy component A with an epoxy value between 0.88 and 0.91, an epoxy component B with an epoxy value between 0.49 and 0.51, an epoxy component C, an epoxy component D and an epoxy component E. More specifically, the epoxy component C is a bisphenol A epoxy resin; the epoxy component D is a phenolphthalein-based polyetherketone toughening agent; and the epoxy component E is 3,3'-diaminodiphenyl sulfone.

[0054] The epoxy values ​​of epoxy A component and epoxy B component are between 0.88-0.91 and 0.49-0.51 respectively, which reflect the crosslinking density and chemical reactivity of the resin. Higher epoxy values ​​generally indicate higher crosslinking density, which helps to improve the hardness and heat resistance of the resin, while possibly affecting the fluidity and processability of the resin.

[0055] Among them, the epoxy C component (bisphenol A type epoxy resin) is usually used as the main crosslinking agent in composite materials. This type of epoxy resin has good heat resistance and chemical stability, which helps to improve the durability and thermal performance of the composite material.

[0056] Among them, epoxy D component (phenolphthalein polyetherketone toughening agent) is mainly used to improve the toughness and impact resistance of the resin. This type of toughening agent can absorb energy when the material is impacted or vibrated, reduce the brittle failure of the composite material, and increase its service life.

[0057] Among them, epoxy E component (3,3'-diaminodiphenyl sulfone) is usually used as a curing agent or hardener in the resin. It plays an important role in the curing process of the composite material, helping to form a stable chemical bond structure between the epoxy resin and the carbon fiber, thereby improving the mechanical properties and durability of the composite material.

[0058] It can be seen that the GME223 resin described in this application can effectively adjust the mechanical properties, heat resistance, durability and processing properties of the composite material through the precise ratio and selection of its various components, so that the final carbon fiber composite material has excellent comprehensive properties and is suitable for various high-demand engineering and aerospace applications.

[0059] In some embodiments, the epoxy A component is a trifunctional m-aminophenol triglycidyl epoxy resin, and the epoxy B component is a trifunctional o-cresol glycidyl ether epoxy resin.

[0060] It should be noted that the epoxy A component (m-aminophenol tris-epoxypropyl epoxy resin) generally has a high crosslink density and chemical reactivity because it is a trifunctional resin. This makes the epoxy A component very suitable as the main curing agent or hardener for improving the mechanical and thermal properties of the composite material. Its high crosslinking ability helps to improve the durability and anti-aging properties of the composite material.

[0061] Epoxy B component (o-cresol glycidyl ether epoxy resin) is usually selected as a toughening agent or a component that provides flexibility in epoxy systems. Its function is to increase the toughness and impact resistance of the composite material, thereby reducing the brittle failure of the material when subjected to force. The use of this component helps to improve the performance of the composite material under dynamic loads, and may also improve its processing performance and wear resistance.

[0062] Therefore, the precise ratio and selection of epoxy A component and epoxy B component can significantly affect the comprehensive performance of the composite material, including strength, durability, toughness, processing and service life. Their reasonable configuration can optimize the characteristics of the composite material according to specific application requirements, so that it can play the best effect in various engineering fields and high-end applications.

[0063] As some optional embodiments of the present application, the medium-strength carbon fiber composite material has a fiber surface density setting range of 132±4 g / ㎡ and a resin content of 33±3%; and is prepared by hot melt coating and hot melt dipping methods.

[0064] First, the fiber surface density is set at 132±4g / ㎡, which means that the weight of carbon fiber is between 128g and 136g per square meter. This setting affects the final density and mechanical properties of the composite material, and is usually used to control the lightweight characteristics and strength requirements of the composite material. Secondly, the resin content is set to 33±3%, which specifies the proportion of resin in the composite material. Appropriate resin content is essential to ensure good impregnation and bonding between carbon fiber and resin, which directly affects the mechanical properties, durability and thermal properties of the material. Furthermore, hot melt coating and hot melt dipping are used for preparation. These methods are common composite material preparation processes used to fully combine and cure the resin with carbon fiber prepreg. The hot melt coating method usually involves coating hot melt resin on the surface of carbon fiber, while the hot melt dipping method is to achieve full impregnation and curing of the resin by impregnating the carbon fiber preform.

[0065] That is, by setting the appropriate fiber surface density and resin content, and adopting effective preparation methods such as hot melt coating and hot melt dipping, it is possible to ensure that medium-strength carbon fiber composites have consistent quality and excellent mechanical properties. The selection of these parameters and preparation methods directly affects the structural integrity, durability and performance stability of the composite material, enabling it to meet the requirements of complex engineering and aerospace applications.

[0066] As some optional embodiments of the present application, the T1100-12K fiber density is 1.76 g / cm 3 , linear density 0.414g / m, tensile strength 7020MPa, tensile modulus 315GPa, and elongation at break 2.23%.

[0067] First, the density of T1100-12K carbon fiber is 1.76g / cm 3 . This parameter refers to the mass of fiber per cubic centimeter, which affects the density and weight of the overall composite material. High density usually means that the mass of the fiber itself is large, so less fiber is needed to achieve a certain strength requirement, which helps lightweight design. Secondly, the linear density of T1100-12K carbon fiber is 0.414g / m, that is, the mass of fiber per meter length. Linear density is an important indicator for evaluating fiber fineness and the uniformity of fiber distribution in composite materials, which affects the mechanical properties and process properties of composite materials. Furthermore, the tensile strength is 7020MPa. Tensile strength is the ability of a material to resist tensile force, indicating the maximum load-bearing capacity of the fiber when it is stressed. High tensile strength means that the fiber can provide higher strength and durability under tensile load; the tensile modulus is 315GPa. The tensile modulus (or elastic modulus) is a measure of the stiffness and elastic recovery ability of a material when it is stressed, indicating the rigidity of the fiber during stretching. A high tensile modulus usually means that the material is less deformed after being stressed and has better shape retention; the elongation at break is 2.23%. Elongation at break is the maximum amount of stretch a material can withstand during stretching, and is usually related to the toughness and durability of the material. A low elongation at break may mean that the material does not deform much when it breaks, but may lack a certain degree of plasticity.

[0068] It can be seen that T1100-12K carbon fiber provides a good mechanical performance foundation for composite materials with its high density, excellent tensile strength and modulus, and moderate elongation at break. These performance parameters can affect the strength, rigidity, durability and overall performance of the material when preparing medium-strength carbon fiber composite materials, making it suitable for fields requiring high strength and lightweight design, such as aerospace, automotive industry and sports equipment manufacturing.

[0069] On the other hand, the embodiment of the present application further provides: a method for preparing the medium-strength carbon fiber composite material as described above, comprising the following steps:

[0070] After T1100-12K T1100 carbon fiber and GME223 resin are treated by hot melt coating and hot melt dipping; the assembled sealing bag after prepreg stacking is leak-checked, and then a vacuum pressure of ≤-0.90Bar is applied; the tank temperature is set to rise at a rate of 2℃ / min to 135±2℃; while heating, the pressure is set to 6.5±0.2Bar for 10 minutes; when the leading thermocouple reaches 130℃, the timing is started to keep the temperature constant for 90±5min; after the constant temperature is ended, the tank temperature is set to rise at a rate of 2℃ / min to 181±2℃; when the lagging thermocouple is heated to 177℃, the timing is started to keep the temperature constant for 180min±5min; the cooling rate is set to be ≤1.5℃ / min, and when the slowest thermocouple temperature drops to 60℃, the pressure and vacuum are released and the tank is taken out.

[0071] This preparation method shows many technical advances and advantages in the preparation of medium-strength carbon fiber composites:

[0072] Using hot melt coating and hot melt dipping to process carbon fiber and resin can ensure that the resin fully impregnates the carbon fiber and improves the interfacial bonding strength of the composite material. Compared with traditional manual or static dipping, these methods can distribute the resin more evenly, reduce the possibility of bubbles and defects, and thus improve the strength and durability of the material.

[0073] Controlling the temperature rise and fall rate and the constant temperature time is very important. In this method, a precise heating rate and temperature range, such as a heating rate of 2°C / min and a specified constant temperature time, is used to ensure the complete reaction of the resin during the curing process. Especially in the high temperature constant temperature stage (such as 181±2°C), by extending the curing time (180min±5min), it helps to increase the cross-linking degree of the resin, thereby improving the thermal stability and mechanical properties of the composite material.

[0074] Applying vacuum pressure ≤-0.90Bar during the entire preparation process helps to remove air and bubbles during the resin impregnation process and ensure good contact between the resin and the carbon fiber. At the same time, during the heating and pressurization stage (6.5±0.2Bar), the permeability of the resin and the fixation of the carbon fiber are increased, further improving the density and mechanical properties of the composite material.

[0075] The cooling rate (≤1.5℃ / min) and temperature control (pressure and vacuum are released after reaching 60℃) in the final stage ensure that the composite material will not produce stress or deformation due to excessive temperature changes during demolding. This precise control helps maintain the shape and dimensional stability of the composite material and reduce the scrap rate in subsequent processing.

[0076] In summary, this preparation method significantly improves the preparation efficiency, quality and performance stability of medium-strength carbon fiber composites by combining advanced material processing technology and precise process control. These technological advances can not only meet the industrial demand for high-performance composites, but also help promote the widespread application of composites in aerospace, automotive and other fields.

[0077] Wherein, the hot melt glue coating method comprises the following steps:

[0078] The resin matrix is ​​placed on a heat-conducting belt to soften the resin matrix into a resin melt; the resin melt is introduced into the glue groove between the glue coating roller and the metering roller through the heat-conducting belt, and the resin melt is evenly coated on the release paper through the glue coating process, and the glue coating accuracy is controlled by the β instrument. After passing the test, the paper is rolled up for standby use. The glue coating process includes: a maximum glue coating speed of 2m / min, a gap between the glue coating and metering rollers of 0.10 to 0.12mm, a setting temperature of the glue coating roller of 70°C, a setting temperature of the melt plate of 80°C, a setting temperature of the cooling roller of 16°C, and a setting weight of the glue coating machine of 32.5g / m 2 .

[0079] It should be noted that the resin matrix is ​​placed on the heat conductive belt, softened into a resin melt, and the resin melt is introduced into the glue groove between the glue coating roller and the metering roller through the heat conductive belt. This step ensures that the resin can be evenly introduced into the glue groove of the glue coating roller at an ideal temperature and pressure, providing a basis for subsequent uniform glue coating. The glue coating process includes a series of precise parameter settings, such as the maximum glue coating speed, the gap between the glue coating roller and the metering roller, the set temperature of each roller, and the set gram weight of the glue coating machine. The precise control of these parameters ensures that the resin melt can be evenly coated on the release paper at a specified gram weight, thereby ensuring the uniformity and quality stability of the composite material. The β instrument is used to detect and control the amount of glue coating to ensure that the accuracy of the amount of glue coating meets the requirements. This high-precision control can effectively reduce waste and unevenness in the glue coating process and improve the utilization rate and consistency of materials. By setting reasonable process parameters and using advanced instruments and equipment, such as glue coating machines and β instruments, this method not only improves production efficiency (such as maximum glue coating speed and set gram weight), but also significantly improves the quality stability of the product. Stable temperature control and precise glue application amount ensure the consistency of composite materials in performance and appearance.

[0080] In summary, this hot melt coating method effectively improves the preparation quality and production efficiency of medium-strength carbon fiber composites by optimizing the technical details in the resin melting, introduction and coating process. These technological advances are not only suitable for the preparation of high-performance materials, but also can meet the industry's demand for high precision and high performance of composite materials.

[0081] Wherein, the hot melt dipping method comprises the following steps:

[0082] Set the temperature of heating zone 1 to 65°C, heating zone 2 to 80°C, heating zone 2 to 75°C, cooling zone 2 to 16°C, the gap between the rollers to 0.35-0.40mm, and the dipping speed to 1-2g / m 2 , the T1100 grade reinforced carbon fiber is spread.

[0083] It should be noted that by setting the precise temperatures of the heating and cooling zones, for example, heating zone 1 is set to 65°C, heating zone 2 is set to 80°C and 75°C, and cooling zone 2 is set to 16°C, the temperature of the fiber and resin can be precisely controlled. This precise temperature control is critical to the melting and impregnation process of the resin, and helps to maintain the stability and consistency of the preparation process. The gap between the rollers is set to 0.35-0.40mm. Precise control within this range can ensure uniform coating between the resin and the fiber during the impregnation process, while avoiding the use of too much or too little resin. Appropriate roller gap is one of the important factors to ensure product quality and stable performance. The impregnation speed is set to 1-2g / m 2 , showing the fine control of the amount of resin used during the impregnation process. This precise control of the impregnation speed not only allows for economical use of the resin, but also helps ensure an ideal combination of fiber and resin, improving the mechanical properties and durability of the composite material. T1100 grade reinforced carbon fibers are typically used in applications that require high strength and light weight, such as the aerospace and automotive industries. This hot melt impregnation method can effectively process this type of high-performance fiber by optimizing parameter settings, ensuring that the composite material has excellent performance and stable quality.

[0084] In summary, this hot melt impregnation method is suitable for processing the yarn spreading process of T1100 grade reinforced carbon fiber by precisely controlling the temperature, roller gap and impregnation speed, thereby improving the efficiency and quality stability in the preparation process of composite materials. These technological advances not only help meet the preparation needs of high-performance materials, but also enhance the dominant position of products in market competition.

[0085] As some optional embodiments of the present application, the GME223 resin is prepared by the following steps: 60 to 80 parts of epoxy component A, 20 to 30 parts of epoxy component B, and 4 to 8 parts of epoxy component C are added to a reaction kettle and mixed evenly at 90°C; then 4 to 6 parts of epoxy component D are added and stirred at 90°C for 15 to 30 minutes to mix evenly;

[0086] After heating to 135°C, stir and heat for 50 to 80 minutes to mix evenly; cool to 90°C, add 32 to 35 parts of epoxy E component, and stir for 10 to 30 minutes;

[0087] The mixture was cooled to 75° C., 1 to 3 parts of epoxy E component were added, and the mixture was stirred for 15 to 30 minutes to be uniformly mixed; after cooling to room temperature, GME223 resin was obtained.

[0088] In order to facilitate the understanding of the technical solution described in the present application by those skilled in the art, the technical solution described in the present application is explained in detail below in combination with specific implementation methods:

[0089] Embodiment 1

[0090] 1) Prepare a high temperature epoxy resin GME223

[0091] High temperature epoxy resin includes five components: Component A: trifunctional m-aminophenol triglycidyl epoxy resin, brown liquid, epoxy value between 0.88-0.91. Component B: trifunctional o-cresol aldehyde glycidyl ether epoxy resin, colorless to yellow transparent solid, epoxy value between 0.49-0.51. Component C: bisphenol A epoxy resin, white solid; Component D: phenolphthalein polyether ketone toughening agent, white solid powder, particle size ≤45μm; Component E: 3,3'-diaminodiphenyl sulfone, white powder, particle size ≤10μm.

[0092] High temperature epoxy resin preparation process:

[0093] a) adding 60-80 parts of m-aminophenol triglycidyl epoxy resin, 20-30 parts of o-cresol glycidyl ether epoxy resin and 4-8 parts of bisphenol A epoxy resin into a reaction kettle, and mixing them uniformly at 90° C.; then adding 4-6 parts of phenolphthalein polyether ketone, and stirring at 90° C. for 15-30 minutes to mix them uniformly;

[0094] b) After heating to 135°C, stir and heat for 50 to 80 minutes to mix evenly;

[0095] c) cooling to 90° C., adding 32 to 35 parts of 3,3'-diaminodiphenyl sulfone, and stirring for 10 to 30 minutes;

[0096] d) Cooling to 75° C., adding 1 to 3 parts of phenolphthalein polyetherketone, stirring for 15 to 30 minutes to mix evenly;

[0097] e) After cooling to room temperature, the epoxy resin composition GME223 was obtained.

[0098] The amount of resin configured shall not exceed two-thirds of the reactor volume and shall not be less than one-third of the volume.

[0099] Resin performance test:

[0100] The rheological properties of the resin matrix were measured by MCR101 rheometer (heating rate was 2℃ / min). The viscosity of the resin was low in the low temperature area, the overall viscosity changed relatively slowly, the low viscosity area was wide, and the lowest viscosity was about 1.0Pa.s. The gel time of the resin at 130℃ was measured to be 9.9min. This result is conducive to the good infiltration of the fiber by the resin during the heating process. The thermal properties of the resin matrix were measured by DSC method. The heating rate was 10℃ / min, the thermal enthalpy of the resin matrix was 393.8J / g, and the heat release during the curing process was relatively stable and uniform. The resin was cured according to the curing process of 180℃ / 2.5h, and the relevant properties of the casting were measured. The tensile modulus can reach 4.09GPa, the elongation at break is 1.32%, and the glass transition temperature is 204.9℃. The resin casting has good rigidity and heat resistance.

[0101] Among them, the viscosity-temperature curve of GME223 resin is shown in Figure 1 , the DSC analysis of curing time is shown in Figure 2 , the physical properties and typical mechanical properties are shown in Table 1.

[0102] Table 1 Physical properties and typical mechanical properties of high temperature epoxy resin system

[0103] Test items unit performance Viscosity (75℃) P 384 Gel time (180℃) Min 9.9 Curing starting temperature (10℃ / min) ℃ 178.7 Curing peak temperature (10℃ / min) ℃ 249.1 Curing end temperature (10℃ / min) ℃ 271.7 Melting enthalpy <![CDATA[J.g -1 ]]> 393.8 Tensile modulus GPa 4.09 Tensile Strength MPa 54.1 Elongation at break % 1.32 Impact strength J / mm 19.2 Glass transition temperature ℃ 204.9

[0104] 2) Preparation of T1100 grade carbon fiber reinforced high-strength medium-mode prepreg

[0105] The fiber surface density of T1100 high-strength medium-mold prepreg is set within the range of 132±4g / ㎡ and the resin content is 33±3%. The prepreg is prepared by a two-step hot melt method (hot melt coating + hot melt dipping) molding process.

[0106] Hot melt glue coating: Place the resin matrix of the specified shape on the preheated guide belt, whose temperature is enough to soften the resin and turn it into a fluid. The resin melt is introduced into the glue groove between the glue coating roller and the metering roller through the hot guide belt. Adjust the process parameters, set the maximum glue coating speed to 2m / min, the gap between the glue coating and metering rollers to 0.10-0.12mm, the setting temperature of the glue coating roller to 70℃, the setting temperature of the melt plate to 80℃, the setting temperature of the cooling roller to 16℃, and the setting weight of the glue coating machine to 32.5g / m 2 The glue coating method adopts direct coating method, and the release paper type adopts release paper with strong release force such as CCK / Taibo. The resin matrix is ​​evenly coated on the release paper, and the accuracy of the glue coating is controlled by β instrument detection. After passing the test, it is rolled up for standby use.

[0107] Hot melt dipping: T1100-12K fiber is used as T1100 grade reinforced carbon fiber with a density of 1.76g / cm 3, linear density 0.414g / m, tensile strength 7020MPa, tensile modulus 315GPa, elongation at break 2.23%. T1100-12K fiber was spread. The temperature of heating zone 1 was set at 65℃, heating zone 2 was set at 80℃, heating zone 2 was set at 75℃, cooling zone 2 was set at 16℃, the gap between the pressure rollers was 0.35-0.40mm, and the dipping speed was 1-2g / m 2 .

[0108] The fiber surface density of T1100 grade carbon fiber reinforced high-strength medium-modulus prepreg is 134g / ㎡, the resin content is 32.3%, and the resin fluidity is 11%, which meets the set requirements.

[0109] 3) Curing and performance testing of T1100 high-strength medium-mold prepreg

[0110] When T1100 grade high-strength medium-mold prepregs were stacked, it was found that the prepregs could not only bond to each other but also be well separated from the release paper and PE film.

[0111] Molding process such as Figure 3 As shown, after leak detection of the assembled sealing bag after the prepreg is laid, a vacuum pressure of ≤-0.90Bar is applied; the tank temperature is set to rise at a rate of 2°C / min to 135±2°C; while heating, the pressure is set to 6.5±0.2Bar for 10 minutes; when the leading thermocouple reaches 130°C, the timing of the constant temperature is started for 90±5min; after the constant temperature is ended, the tank temperature is set to rise at a rate of 2°C / min to 181±2°C; when the lagging thermocouple is heated to 177°C, the timing of the constant temperature is started for 180min±5min; the temperature is set to fall at a rate of ≤1.5°C / min, and when the slowest thermocouple temperature drops to 60°C, the pressure and vacuum are released, and the composite material is taken out of the tank to obtain.

[0112] Composite material performance test:

[0113] The single layer thickness of the prepreg after curing is 0.124mm, and the non-destructive test is qualified with a thickness deviation of 3%.

[0114] Table 2 Thickness test of laminate after curing of high temperature and high strength medium mold prepreg

[0115]

[0116] The average interlaminar shear strength of the composite material is 98MPa and the minimum is 87MPa. After molding, the composite material has good interlaminar bonding. The composite material has good mechanical properties, with an average tensile strength of 3003MPa and a minimum of 2734MPa; an average tensile modulus of 217GPa and a minimum of 206GPa; an average compressive strength of 1437MPa and a minimum of 1328MPa; an average compression modulus of 189GPa and a minimum of 184GPa. It helps to meet the requirements of lightweight, high strength and high stiffness of composite structures.

[0117] Table 3 Properties of composite materials after curing of high temperature and high strength medium mold prepreg

[0118]

[0119] Embodiment 2

[0120] The GME223 resin system is prepared according to the following steps:

[0121] a) Add 70 parts of m-aminophenol triglycidyl epoxy resin, 15 parts of o-cresol glycidyl ether epoxy resin, and 5 parts of bisphenol A epoxy resin into a reaction kettle, and stir at 90° C. for 20 minutes; add 5 parts of phenolphthalein polyether ketone and 2 parts of polyether sulfone, and stir at 90° C. for 15 minutes to mix;

[0122] b) After heating to 130°C, stir and heat for 30 to 50 minutes;

[0123] c) cooling to 90° C., adding 34 parts of 3,3'-diaminodiphenyl sulfone, and stirring for 20 minutes;

[0124] d) cooling to 75° C., adding 5 parts of phenolphthalein polyetherketone, and stirring for 25 minutes;

[0125] e) After cooling to room temperature, the epoxy resin composition GME223 was obtained.

[0126] Embodiment 3

[0127] The GME223 resin system is prepared according to the following steps:

[0128] a) adding 60 parts of m-aminophenol triglycidyl epoxy resin, 35 parts of o-cresol glycidyl ether epoxy resin and 5 parts of bisphenol A epoxy resin into a reaction kettle and mixing them uniformly at 90° C.; then adding 4 to 6 parts of phenolphthalein polyether ketone and stirring them at 90° C. for 15 to 30 minutes to mix them uniformly;

[0129] b) After heating to 135°C, stir and heat for 50 to 80 minutes to mix evenly;

[0130] c) cooling to 90° C., adding 32 to 35 parts of 4,4'-diaminodiphenyl sulfone, and stirring for 10 to 30 minutes;

[0131] d) Cooling to 75° C., adding 1 to 3 parts of phenolphthalein polyetherketone, stirring for 15 to 30 minutes to mix evenly;

[0132] e) After cooling to room temperature, the epoxy resin composition GME223 was obtained.

[0133] GME223 high temperature epoxy resin is suitable for the two-step hot melt method to produce T1100 grade carbon fiber prepreg. The prepregs can be bonded to each other and can be well separated from the release paper and PE film. After forming the composite material, it has good interlayer bonding and the interlayer shear strength can reach 98MPa. The average tensile strength of the composite material is 3003MPa, the tensile modulus is 217GPa, the compressive strength is 1437MPa, and the compression modulus is 189GPa. The tensile and compressive strength of the composite material is about 20% higher than that of the T700 grade series composite material, and the tensile modulus and compression modulus are about 30% higher.

[0134] In this application, m-aminophenol triglycidyl epoxy resin, o-cresol glycidyl ether epoxy resin, bisphenol A epoxy resin, phenolphthalein polyether ketone, and diaminodiphenyl sulfone are formulated into a GME223 high-temperature epoxy resin system through appropriate proportions. T1100-grade carbon fiber is used as a reinforcing material, and a high-temperature and high-strength medium-mold prepreg is prepared by a hot melt method. A zero-adhesion pressurization molding process for T1100-grade carbon fiber prepreg is designed and determined, and a high-performance composite material component is prepared by an autoclave method. The present invention provides a method for preparing a high-temperature epoxy resin, a method for preparing a T1100-grade carbon fiber reinforced high-strength medium-mold prepreg, and a composite material, which are of high value in meeting the requirements of lightweight, high strength, and high stiffness of aircraft structures.

[0135] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A medium-strength carbon fiber composite material, characterized in that: The medium-strength carbon fiber composite material is prepared by using T1100-12K carbon fiber as a reinforcing material and GME223 resin as a matrix material; The average interlaminar shear strength of the carbon fiber composite material is 98 MPa, and the minimum is 87 MPa; The average tensile strength of the carbon fiber composite material is 3003 MPa, and the minimum is 2734 MPa; The average tensile modulus of the carbon fiber composite material is 217 GPa, and the minimum is 206 GPa; The average compressive strength of the carbon fiber composite material is 1437 MPa, and the minimum is 1328 MPa; The average compression modulus of the carbon fiber composite material is 189 GPa, and the minimum is 184 GPa.

2. The medium-strength carbon fiber composite material according to claim 1, characterized in that: The GME223 resin comprises: an epoxy A component with an epoxy value between 0.88 and 0.91, an epoxy B component with an epoxy value between 0.49 and 0.51, an epoxy C component, an epoxy D component and an epoxy E component. The epoxy C component is bisphenol A type epoxy resin; the epoxy D component is phenolphthalein based polyetherketone toughening agent; and the epoxy E component is 3,3'-diaminodiphenyl sulfone.

3. The medium-strength carbon fiber composite material according to claim 2, characterized in that: The epoxy component A is a trifunctional m-aminophenol triglycidyl epoxy resin.

4. The medium-strength carbon fiber composite material according to claim 2, characterized in that: The epoxy B component is a trifunctional o-cresol glycidyl ether type epoxy resin.

5. The medium-strength carbon fiber composite material according to claim 1, characterized in that: The medium-strength carbon fiber composite material has a fiber surface density setting range of 132±4 g / ㎡ and a resin content of 33±3%; it is prepared by a hot-melt coating method and a hot-melt dipping method.

6. The medium-strength carbon fiber composite material according to claim 5, characterized in that: The T1100-12K fiber density is 1.76 g / cm 3 , linear density 0.414g / m, tensile strength 7020MPa, tensile modulus 315GPa, and elongation at break 2.23%.

7. A method for preparing the medium-strength carbon fiber composite material according to any one of claims 1 to 6, characterized in that: The following steps are involved: T1100-12K carbon fiber and GME223 resin are treated by hot melt coating and hot melt dipping methods; the assembled sealing bag after prepreg stacking is leak-checked, and then a vacuum pressure of ≤-0.90Bar is applied; the tank temperature is set to rise at a rate of 2℃ / min to 135±2℃; while heating, the pressure is set to 6.5±0.2Bar for 10 minutes; when the leading thermocouple reaches 130℃, the timing is started to keep the temperature constant for 90±5min; after the constant temperature is over, the tank temperature is set to rise at a rate of 2℃ / min to 181±2℃; when the lagging thermocouple is heated to 177℃, the timing is started to keep the temperature constant for 180min±5min; the cooling rate is set to be ≤1.5℃ / min, and when the slowest thermocouple temperature drops to 60℃, the pressure and vacuum are released and the tank is taken out.

8. The method for preparing the medium-strength carbon fiber composite material according to claim 7, characterized in that: The hot melt glue coating method comprises the following steps: The resin matrix is ​​placed on a heat-conductive belt to soften the resin matrix into a resin melt; the resin melt is introduced into the glue groove between the glue coating roller and the metering roller through the heat-conductive belt, and the resin melt is evenly coated on the release paper through a glue coating process, and the accuracy of the glue coating amount is controlled by a β instrument. After passing the test, the resin is rolled up for standby use.

9. The method for preparing the medium-strength carbon fiber composite material according to claim 8, characterized in that: The gluing process includes: a maximum gluing speed of 2 m / min, a gap between the gluing / metering rollers of 0.10-0.12 mm, a setting temperature of the gluing roller of 70°C, a setting temperature of the melting plate of 80°C, a setting temperature of the cooling roller of 16°C, and a setting weight of the gluing machine of 32.5 g / m 2 .

10. The method for preparing the high-strength mid-mode prepreg according to claim 7, characterized in that: The hot melt dipping method comprises the following steps: Set the temperature of heating zone 1 to 65°C, heating zone 2 to 80°C, heating zone 2 to 75°C, cooling zone 2 to 16°C, the gap between the rollers to 0.35-0.40mm, and the dipping speed to 1-2g / m 2 , the T1100 grade reinforced carbon fiber is spread.

11. The method for preparing the medium-strength carbon fiber composite material according to claim 7, characterized in that: The GME223 resin is prepared by the following steps: Add 60 to 80 parts of epoxy component A, 20 to 30 parts of epoxy component B, and 4 to 8 parts of epoxy component C into a reaction kettle and mix them evenly at 90°C; then add 4 to 6 parts of epoxy component D and stir at 90°C for 15 to 30 minutes to mix evenly; After heating to 135°C, stir and heat for 50 to 80 minutes to mix evenly; cool to 90°C, add 32 to 35 parts of epoxy E component, and stir for 10 to 30 minutes; The mixture was cooled to 75° C., 1 to 3 parts of epoxy E component were added, and the mixture was stirred for 15 to 30 minutes to be uniformly mixed; after cooling to room temperature, GME223 resin was obtained.

Citation Information

Cited By

  • Carbon fiber composite material and preparation method thereof

    CN121362434A