Anti-ultraviolet PC / ABS composite material as well as preparation method and application thereof

By adding anti-ultraviolet agents and compatibilizers to PC/ABS composite materials and adopting melt blending technology, the problem of aging of the car lamp housing under ultraviolet light is solved, and the effect of improving anti-ultraviolet performance and taking into account both mechanical properties is achieved. Simplifies the process and reduces costs.

CN118931146APending Publication Date: 2024-11-12CHANGZHOU XINGYU AUTOMOTIVE LIGHTING SYST CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411183220.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing headlight shell made of PC/ABS composite material accelerates aging under ultraviolet irradiation, resulting in a decrease in strength. The existing UV-resistant improvement methods are costly, complex and difficult.

Method used

Prepared by adding anti-UV agents and compatibilizers to the PC/ABS composite material and using a melt blending process, specifically including polycarbonate, acrylonitrile-butadiene-styrene copolymer, modified tannin, and containing Components such as epoxy groups, styrene-acrylate copolymers, maleic anhydride graft copolymers, stearic acid amides, pentaerythritol stearate and methyl silicone oil are subjected to twin-screw extrusion processing to prepare UV-resistant PC/ABS composite material.

Benefits of technology

It has achieved the improvement of UV resistance, simple process, low cost, and good mechanical properties, reducing the difficulty of preparation and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012807700000091
    Figure BDA0005012807700000091
  • Figure BDA0005012807700000092
    Figure BDA0005012807700000092
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, in particular to an anti-ultraviolet PC / ABS (polycarbonate / acrylonitrile butadiene styrene) composite material as well as a preparation method and application thereof. The anti-ultraviolet PC / ABS composite material is prepared from the following components in parts by weight: 60 to 90 parts of polycarbonate, 10 to 40 parts of acrylonitrile-butadiene-styrene copolymer, 0.5 to 5 parts of anti-ultraviolet agent, 0.5 to 5 parts of compatibilizer, 0.3 to 1 part of antioxidant and 1 to 5 parts of lubricant, wherein the sum of the weight parts of the polycarbonate and the acrylonitrile-butadiene-styrene copolymer is 100 parts. By adding the anti-ultraviolet agent and the compatibilizer, the PC / ABS automobile lamp shell prepared after melt blending has good anti-ultraviolet performance, the process is simple, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to an anti-ultraviolet PC / ABS composite material and a preparation method and application thereof. Background Art

[0002] Polycarbonate (PC for short) is a highly linear thermoplastic polymer material with flexible carbonate groups and rigid benzene ring groups on the main chain. Such a molecular chain structure gives PC materials good rigidity, heat resistance and excellent notched impact resistance. PC and ABS (acrylonitrile-butadiene-styrene copolymer) can combine the excellent properties of both. On the one hand, the heat resistance, impact strength and tensile strength of PC / ABS composite materials are better than ABS. On the other hand, its cost and melt viscosity are lower than PC, and its processing performance is better than PC. The sensitivity of its internal stress and impact strength to the thickness of the product is greatly reduced, and it can be used for car lamp housings.

[0003] The headlight housing is an important part of the entire vehicle lamp. Its main function is to support the lens, circuit board and electronic components inside the lamp. Under ultraviolet radiation, the headlight housing made of existing PC / ABS composite materials will accelerate aging. After aging, the strength of the headlight housing will significantly decrease, affecting the normal use of the headlight and thus adversely affecting driving safety.

[0004] At present, the main method to improve the anti-ultraviolet performance of car lamp materials is to spray UV paint on the surface. UV paint produces free radicals under the irradiation of ultraviolet light, undergoes resin reaction, and forms a paint film that is resistant to ultraviolet light, thereby improving the anti-ultraviolet performance of car lamp materials and making them less prone to aging. In addition, the UV paint film has the advantages of environmental protection, high hardness, wear resistance and high transparency.

[0005] However, spraying UV paint on the surface of the lamp housing has the following disadvantages:

[0006] (1) High cost. The production cost of UV paint is high and the price is relatively expensive;

[0007] (2) High technical requirements. The construction of UV paint requires professional technology and equipment, and also has high requirements for construction personnel;

[0008] (3) The surface of the product sprayed with UV paint has different surface roughness and glossiness. Summary of the invention

[0009] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide an anti-ultraviolet PC / ABS composite material and a preparation method and application thereof. The present invention adds an anti-ultraviolet agent and a compatibilizer, and the PC / ABS lamp housing prepared by melt blending has good anti-ultraviolet performance, and the process is simple and the cost is low.

[0010] The technical solution adopted by the present invention to solve its technical problem is:

[0011] An anti-ultraviolet PC / ABS composite material comprises the following components in parts by weight:

[0012] Polycarbonate 60-90 parts

[0013] 10-40 parts of acrylonitrile-butadiene-styrene copolymer

[0014] 0.5-5 parts of anti-ultraviolet agent

[0015] 0.5~5 parts of extender

[0016] Antioxidant 0.3-1 part

[0017] 1 to 5 parts of lubricant;

[0018] The total weight of the polycarbonate and the acrylonitrile-butadiene-styrene copolymer is 100 parts.

[0019] Furthermore, the polycarbonate is bisphenol A polycarbonate with a molecular weight of 15000 to 45000 g / mol; and the mass percentage of butadiene in the acrylonitrile-butadiene-styrene copolymer is 10 to 40%.

[0020] Furthermore, the anti-ultraviolet agent is modified tannic acid, and the preparation method of the modified tannic acid is as follows:

[0021] The silane coupling agent is dissolved in an acidic solution for hydrolysis, wherein the pH value of the acidic solution is 4.5 to 6.5, and stirred until transparent to obtain a silane coupling agent solution, the silane coupling agent solution is mixed with tannic acid to obtain a mixed solution, the mixed solution is adjusted to be weakly alkaline, wherein the pH value of the mixed solution is 8 to 10, the stirring is continued, the mixture is allowed to stand for stratification, the supernatant is removed, and the mixture is filtered, washed, and dried to obtain modified tannic acid;

[0022] The mass of the silane coupling agent is 0.2-5% of the mass of the tannic acid;

[0023] The stirring temperature of the mixed solution is 25-50° C., and the stirring time is 8-50 hours.

[0024] Silane coupling agent is an important chemical agent, mainly used to improve the interface bonding between inorganic materials and organic materials. Here, it can form chemical bonds or compatibility with organic materials (such as resins, rubbers, etc.), thereby playing a "coupling" role. By adding silane coupling agent, modified tannic acid is obtained, thereby improving the dispersion effect of tannic acid in PC / ABS matrix.

[0025] Furthermore, the silane coupling agent may be one of KH550, KH560 and KH570.

[0026] Furthermore, the compatibilizer is at least one of a styrene-acrylate copolymer containing an epoxy group and a maleic anhydride grafted copolymer.

[0027] Furthermore, the antioxidant is a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris[2,4-di-tert-butylphenyl]phosphite, and the mass ratio of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris[2,4-di-tert-butylphenyl]phosphite is 1:1.

[0028] Furthermore, the lubricant is at least one of stearic acid amide, pentaerythritol stearate and methyl silicone oil.

[0029] A method for preparing the above-mentioned UV-resistant PC / ABS composite material specifically comprises the following steps:

[0030] Step S1, weighing polycarbonate, acrylonitrile-butadiene-styrene copolymer and anti-ultraviolet agent, and drying the above materials in an oven for 12 hours, and then putting them into an aluminum foil bag and sealing them for standby use, to obtain an initial material;

[0031] Step S2, weighing the compatibilizer, antioxidant and antioxidant, and putting them into a high-speed mixer together with the initial material obtained in step S1 for premixing, the premixing time is 15 to 30 minutes, to obtain a premix;

[0032] Step S3, pouring the premix in step S2 into a twin-screw extruder through a barrel. The twin-screw extruder is divided into a preheating section, a shearing section and a mixing section. After the twin-screw extrusion, it is cooled, dried and pelletized to obtain an anti-ultraviolet PC / ABS composite material.

[0033] Furthermore, in step S3, the screw processing temperature ranges from 210 to 250° C., and the screw speed ranges from 80 to 200 rpm.

[0034] An application of the above-mentioned UV-resistant PC / ABS composite material is used to prepare an UV-resistant PC / ABS composite film or an UV-resistant PC / ABS vehicle lamp housing.

[0035] The anti-ultraviolet PC / ABS composite film is used for performance testing after the anti-ultraviolet PC / ABS composite material is hot-pressed into a film, wherein the hot-pressing temperature is 250°C and the pressure is 10MPa.

[0036] The anti-ultraviolet PC / ABS car lamp housing is prepared by adding the anti-ultraviolet PC / ABS composite material into an injection molding machine for melting and then cooling and molding, wherein the injection molding temperature is 220-260° C. and the injection molding pressure is 15-20 MPa.

[0037] The beneficial effects of the present invention are as follows: the present invention has a reasonable design, a simple preparation method, and has the following advantages:

[0038] (1) By adding an anti-ultraviolet agent and a compatibilizer, the PC / ABS composite material prepared after melt blending has good anti-ultraviolet performance, and the process is simple and the cost is low;

[0039] (2) The headlight housing is made of PC / ABS composite material, which improves the anti-ultraviolet performance and has good mechanical properties;

[0040] (3) The difficulty of the preparation process of the UV-resistant PC / ABS lamp housing is reduced, the production efficiency is improved, and the production cost is reduced. DETAILED DESCRIPTION

[0041] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0042] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0043] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Example 1

[0045] A method for preparing an anti-ultraviolet PC / ABS composite material comprises the following steps:

[0046] Step S1, placing 70 parts of polycarbonate, 30 parts of acrylonitrile-butadiene-styrene copolymer, and 1 part of anti-ultraviolet agent in an oven and drying for 12 hours, then placing them in an aluminum foil bag and sealing them for standby use, to obtain an initial material;

[0047] Step S2, adding 1 part of a compatibilizer, 0.3 parts of an antioxidant, 2 parts of a lubricant and the initial material into a high-speed mixer and premixing for 15 minutes to obtain a premix;

[0048] Step S3, adding the premix into the hopper of a twin-screw extruder, and melt-extruded after passing through a preheating section, a shearing section and a mixing section, the corresponding temperatures are 215° C., 240° C., and 225° C., respectively, and the screw speed is 80-200 rpm, and finally cooling, drying, and pelletizing to obtain an anti-UV PC / ABS composite material.

[0049] An anti-ultraviolet PC / ABS composite film is used for performance testing after the anti-ultraviolet PC / ABS composite material is hot-pressed into a film, wherein the hot-pressing temperature is 250° C. and the pressure is 10 MPa.

[0050] An anti-ultraviolet PC / ABS vehicle lamp shell is prepared by adding an anti-ultraviolet PC / ABS composite material into an injection molding machine for melting and then cooling and molding, wherein the injection molding temperature is 250°C and the injection molding pressure is 20MPa.

[0051] Example 2

[0052] A method for preparing an anti-ultraviolet PC / ABS composite material comprises the following steps:

[0053] Step S1, placing 70 parts of polycarbonate, 30 parts of acrylonitrile-butadiene-styrene copolymer, and 2 parts of anti-ultraviolet agent in an oven and drying for 12 hours, then placing them in an aluminum foil bag and sealing them for standby use, to obtain an initial material;

[0054] Step S2, adding 1 part of a compatibilizer, 0.3 parts of an antioxidant, 2 parts of a lubricant and the initial material into a high-speed mixer and premixing for 15 minutes to obtain a premix;

[0055] Step S3, adding the premix into the hopper of a twin-screw extruder, and melt-extruded after passing through a preheating section, a shearing section and a mixing section, the corresponding temperatures are 215° C., 240° C., and 225° C., respectively, and the screw speed is 80-200 rpm, and finally cooling, drying, and pelletizing to obtain an anti-UV PC / ABS composite material.

[0056] An anti-ultraviolet PC / ABS composite film is used for performance testing after the anti-ultraviolet PC / ABS composite material is hot-pressed into a film, wherein the hot-pressing temperature is 250° C. and the pressure is 10 MPa.

[0057] An anti-ultraviolet PC / ABS vehicle lamp shell is prepared by adding an anti-ultraviolet PC / ABS composite material into an injection molding machine for melting and then cooling and molding, wherein the injection molding temperature is 250°C and the injection molding pressure is 20MPa.

[0058] Example 3

[0059] A method for preparing an anti-ultraviolet PC / ABS composite material comprises the following steps:

[0060] Step S1, placing 70 parts of polycarbonate, 30 parts of acrylonitrile-butadiene-styrene copolymer, and 3 parts of anti-ultraviolet agent in an oven and drying for 12 hours, then placing them in an aluminum foil bag and sealing them for standby use, to obtain an initial material;

[0061] Step S2, adding 1 part of a compatibilizer, 0.3 parts of an antioxidant, 2 parts of a lubricant and the initial material into a high-speed mixer and premixing for 15 minutes to obtain a premix;

[0062] Step S3, adding the premix into the hopper of a twin-screw extruder, and melt-extruded after passing through a preheating section, a shearing section and a mixing section, the corresponding temperatures are 215° C., 240° C., and 225° C., respectively, and the screw speed is 80-200 rpm, and finally cooling, drying, and pelletizing to obtain an anti-UV PC / ABS composite material.

[0063] An anti-ultraviolet PC / ABS composite film is used for performance testing after the anti-ultraviolet PC / ABS composite material is hot-pressed into a film, wherein the hot-pressing temperature is 250° C. and the pressure is 10 MPa.

[0064] An anti-ultraviolet PC / ABS vehicle lamp shell is prepared by adding an anti-ultraviolet PC / ABS composite material into an injection molding machine for melting and then cooling and molding, wherein the injection molding temperature is 250°C and the injection molding pressure is 20MPa.

[0065] Example 4

[0066] A method for preparing an anti-ultraviolet PC / ABS composite material comprises the following steps:

[0067] Step S1, placing 70 parts of polycarbonate, 30 parts of acrylonitrile-butadiene-styrene copolymer, and 3 parts of anti-ultraviolet agent in an oven and drying for 12 hours, then placing them in an aluminum foil bag and sealing them for standby use, to obtain an initial material;

[0068] Step S2, adding 0.7 parts of a compatibilizer, 0.3 parts of an antioxidant, and 2 parts of a lubricant and the initial material into a high-speed mixer and premixing for 15 minutes to obtain a premix;

[0069] Step S3, adding the premix into the hopper of a twin-screw extruder, and melt-extruded after passing through a preheating section, a shearing section and a mixing section, the corresponding temperatures are 215° C., 240° C., and 225° C., respectively, and the screw speed is 80-200 rpm, and finally cooling, drying, and pelletizing to obtain an anti-UV PC / ABS composite material.

[0070] An anti-ultraviolet PC / ABS composite film is used for performance testing after the anti-ultraviolet PC / ABS composite material is hot-pressed into a film, wherein the hot-pressing temperature is 250° C. and the pressure is 10 MPa.

[0071] An anti-ultraviolet PC / ABS vehicle lamp shell is prepared by adding an anti-ultraviolet PC / ABS composite material into an injection molding machine for melting and then cooling and molding, wherein the injection molding temperature is 250°C and the injection molding pressure is 20MPa.

[0072] Comparative Example 1

[0073] A method for preparing a PC / ABS composite material comprises the following steps:

[0074] 70 parts of polycarbonate and 30 parts of acrylonitrile-butadiene-styrene copolymer are placed in an oven for drying for 12 hours, and then sealed in an aluminum foil bag for standby use; 0.3 parts of an antioxidant and 2 parts of a lubricant are added into a high-speed mixer together with the dried 70 parts of polycarbonate and 30 parts of acrylonitrile-butadiene-styrene copolymer for premixing for 15 minutes to obtain a premix; the premix is ​​added into a hopper of a twin-screw extruder, and melt-extruded after passing through a preheating section, a shearing section and a mixing section, and the corresponding temperatures are 215°C, 240°C, and 225°C, respectively, and the screw speed is 80-200rpm, and finally the PC / ABS composite material is obtained through cooling, drying, and pelletizing.

[0075] The PC / ABS composite material was hot-pressed into a film for performance testing, wherein the hot-pressing temperature was 250°C and the pressure was 10 MPa.

[0076] The PC / ABS composite material is added into an injection molding machine for melting and then cooled to form a PC / ABS headlight housing, wherein the injection molding temperature is 250° C. and the injection molding pressure is 20 MPa.

[0077] Comparative Example 2

[0078] A method for preparing a PC / ABS composite material comprises the following steps:

[0079] 70 parts of polycarbonate, 30 parts of acrylonitrile-butadiene-styrene copolymer and 1 part of anti-ultraviolet agent are placed in an oven for drying for 12 hours and then sealed in an aluminum foil bag for standby use; 0.3 parts of antioxidant, 2 parts of lubricant, 70 parts of dried polycarbonate, 30 parts of acrylonitrile-butadiene-styrene copolymer and 1 part of anti-ultraviolet agent are added into a high-speed mixer for premixing for 15 minutes to obtain a premix; the premix is ​​added into a hopper of a twin-screw extruder, and melt-extruded after passing through a preheating section, a shearing section and a mixing section, and the corresponding temperatures are 215°C, 240°C and 225°C, respectively, and the screw speed is 80-200rpm; finally, the PC / ABS composite material is obtained through cooling, drying and pelletizing.

[0080] The PC / ABS composite material was hot-pressed into a film for performance testing, wherein the hot-pressing temperature was 250°C and the pressure was 10 MPa.

[0081] The PC / ABS composite material is added into an injection molding machine for melting and then cooled to form, so as to obtain an anti-ultraviolet PC / ABS lamp housing, wherein the injection molding temperature is 250° C. and the injection molding pressure is 20 MPa.

[0082] The weight proportions of the components of Examples 1 to 4, Comparative Example 1 and Comparative Example 2 are specifically shown in Table 1.

[0083] Table 1 Component weight parts of Examples 1 to 4, Comparative Examples 1 and 2

[0084]

[0085]

[0086] The composite membranes prepared in Examples 1 to 4, Comparative Examples 1 and 2 were subjected to performance tests, and the test results are shown in Table 2.

[0087] Table 2 Test results of Examples 1 to 4, Comparative Example 1 and Comparative Example 2

[0088]

[0089] It can be seen from Table 2 that the anti-ultraviolet performance of PC / ABS composites is improved after adding the anti-ultraviolet agent. On this basis, adding the compatibilizer can further improve the mechanical properties and anti-ultraviolet performance of PC / ABS composites. As the mass fraction of the anti-ultraviolet agent gradually increases, the anti-ultraviolet performance of PC / ABS composites continues to improve. When the mass fraction of the anti-ultraviolet agent is the same, changing the mass fraction of the compatibilizer can also further improve the anti-ultraviolet performance and mechanical properties of the PC / ABS composite.

[0090] The invention has reasonable design and simple preparation method and has the following advantages:

[0091] (1) By adding an anti-ultraviolet agent and a compatibilizer, the PC / ABS composite material prepared after melt blending has good anti-ultraviolet performance, and the process is simple and the cost is low;

[0092] (2) The headlight housing is made of PC / ABS composite material, which improves the anti-ultraviolet performance and has good mechanical properties;

[0093] (3) The difficulty of the preparation process of the UV-resistant PC / ABS lamp housing is reduced, the production efficiency is improved, and the production cost is reduced.

[0094] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An anti-ultraviolet PC / ABS composite material, characterized in that: By weight, it includes the following components: Polycarbonate 60-90 parts 10-40 parts of acrylonitrile-butadiene-styrene copolymer 0.5-5 parts of anti-ultraviolet agent 0.5~5 parts of extender Antioxidant 0.3-1 part 1 to 5 parts of lubricant; The total weight of the polycarbonate and the acrylonitrile-butadiene-styrene copolymer is 100 parts.

2. The UV-resistant PC / ABS composite material according to claim 1, characterized in that: The polycarbonate is bisphenol A type polycarbonate with a molecular weight of 15000-45000 g / mol; the mass percentage of butadiene in the acrylonitrile-butadiene-styrene copolymer is 10-40%.

3. The UV-resistant PC / ABS composite material according to claim 1, characterized in that: The anti-ultraviolet agent is modified tannic acid, and the preparation method of the modified tannic acid is as follows: The silane coupling agent is dissolved in an acidic solution for hydrolysis, wherein the pH value of the acidic solution is 4.5 to 6.5, and stirred until transparent to obtain a silane coupling agent solution, the silane coupling agent solution is mixed with tannic acid to obtain a mixed solution, the mixed solution is adjusted to be weakly alkaline, wherein the pH value of the mixed solution is 8 to 10, the stirring is continued, the mixture is allowed to stand for stratification, the supernatant is removed, and the mixture is filtered, washed, and dried to obtain modified tannic acid; The mass of the silane coupling agent is 0.2-5% of the mass of tannic acid; The stirring temperature of the mixed solution is 25-50° C., and the stirring time is 8-50 hours.

4. The UV-resistant PC / ABS composite material according to claim 3, characterized in that: The silane coupling agent may be one of KH550, KH560 and KH570.

5. The UV-resistant PC / ABS composite material according to claim 1, characterized in that: The compatibilizer is at least one of a styrene-acrylate copolymer containing epoxy groups and a maleic anhydride grafted copolymer.

6. The UV-resistant PC / ABS composite material according to claim 1, characterized in that: The antioxidant is a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris[2,4-di-tert-butylphenyl]phosphite, and the mass ratio of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris[2,4-di-tert-butylphenyl]phosphite is 1:

1.

7. The UV-resistant PC / ABS composite material according to claim 1, characterized in that: The lubricant is at least one of stearic acid amide, pentaerythritol stearate and methyl silicone oil.

8. A method for preparing the UV-resistant PC / ABS composite material according to any one of claims 1 to 7, characterized in that: The specific steps include: Step S1, weighing polycarbonate, acrylonitrile-butadiene-styrene copolymer and anti-ultraviolet agent, and drying the above materials in an oven for 12 hours, and then putting them into an aluminum foil bag and sealing them for standby use, to obtain an initial material; Step S2, weighing the compatibilizer, antioxidant and antioxidant, and putting them into a high-speed mixer together with the initial material obtained in step S1 for premixing, the premixing time is 15 to 30 minutes, to obtain a premix; Step S3, pouring the premix in step S2 into a twin-screw extruder through a barrel. The twin-screw extruder is divided into a preheating section, a shearing section and a mixing section. After the twin-screw extrusion, it is cooled, dried and pelletized to obtain an anti-ultraviolet PC / ABS composite material.

9. The method for preparing the UV-resistant PC / ABS composite material according to claim 8, characterized in that: In step S3, the screw processing temperature ranges from 210 to 250° C., and the screw speed ranges from 80 to 200 rpm.

10. An application of the UV-resistant PC / ABS composite material according to any one of claims 1 to 7, characterized in that: Used to prepare UV-resistant PC / ABS composite films or UV-resistant PC / ABS car lamp housings.

Citation Information

Cited By

  • Anti-aging decorative frame for car lamp and preparation method of anti-aging decorative frame

    CN119978755A

  • Aging-resistant decorative frame for vehicle lamp and preparation method thereof

    CN119978755B