Flame-retardant PC plastic and preparation method thereof

Through the surface modification and cross-linking reaction of polycarbonate resin, N, P and Si collaborative flame retardant structures are formed, which solves the problem of insufficient performance of polycarbonate in the field of high flame retardant requirements, and significantly improves the flame retardant performance and stability.

CN118931148AInactive Publication Date: 2024-11-12LIUYANG CONSOLIDATED HARDWARE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226115.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In some areas with high flame retardant requirements, polycarbonate has insufficient flame retardant performance and is difficult to meet stricter application needs.

Method used

By surface modification and modification of the polycarbonate resin, free amino groups are introduced, and reacted with compounds such as p-chlorophenyltrimethoxysilane and triphenylphosphine oxide to form a crosslinking system, KCl nanoparticles are added to form N and P , Si collaborative flame retardant structure to improve flame retardant performance.

Benefits of technology

It significantly improves the flame retardant performance of polycarbonate, enhances stability and thermal stability, reduces the impact of flame retardant on transparency and light transmittance, and achieves a higher level of flame retardant effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931148A_ABST
    Figure CN118931148A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of plastics, and discloses a flame-retardant PC plastic and a preparation method thereof. The preparation method of the flame-retardant PC plastic comprises the following steps: adding PC resin into an ethanol solution of ethylenediamine, and reacting to obtain surface modified PC resin; the preparation method comprises the following steps: mixing p-chlorophenyltrimethoxysilane dispersion liquid with a KCl aqueous solution, reacting, dropwise adding a catalyst solution, and reacting to obtain a compound A; mixing the intermediate with stannous chloride dehydrate, adding ethanol and concentrated hydrochloric acid, adjusting the pH value, and standing to obtain a compound B; and mixing the surface modified PC resin, the compound B, toluene and triethylamine, dropwise adding the dispersion liquid of the compound A, and reacting to obtain the flame-retardant PC resin. And adding the antioxidant, the color master batch, the lubricant and the hydrolysis-resistant agent into the flame-retardant PC resin, then adding the epoxy resin, the thermoplastic polyurethane elastomer and the gelatin, and carrying out injection molding to obtain the flame-retardant PC plastic. The flame-retardant PC plastic obtained by the method disclosed by the invention is excellent in flame retardance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, in particular to a flame retardant PC plastic and a preparation method thereof. Background Art

[0002] Polycarbonate (PC) is a highly transparent, colorless, non-toxic, odorless amorphous thermoplastic resin. It can be divided into aromatic, aliphatic, aliphatic, and aromatic according to the structure of the ester group in the molecular chain. Due to the requirements for mechanical properties, only aromatic polycarbonate has been industrialized. Polycarbonate has excellent comprehensive performance, with balanced mechanical properties, good dimensional stability, easy coloring, excellent aging resistance and electrical insulation properties. Due to the excellent performance of polycarbonate, it is widely used in electronics, electrical appliances, aerospace, machinery, automobile textiles, light industry and construction industries. As an engineering plastic, polycarbonate itself has good flame retardant properties, vertical combustion can reach UL-94V2 level, and the limiting oxygen index reaches 28%. However, if it is used in other fields with higher flame retardant requirements such as electronics, electrical and architectural decoration, polycarbonate still needs to be flame retardant. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a method for preparing a flame retardant PC plastic, comprising the following steps:

[0004] Step (1) adding PC resin to an ethanol solution of ethylenediamine, heating, soaking and reacting in a sealed environment, cooling, filtering, washing, and drying to obtain a surface-modified PC resin;

[0005] In the above reaction process, the amino group in ethylenediamine reacts with the ester bond in the PC resin to form a carbamate bond, leaving free amino groups on the surface of the PC resin that can be used for subsequent reactions.

[0006] Step (2) mixing a p-chlorophenyltrimethoxysilane dispersion with a KCl aqueous solution, heating, reacting, then dropping a catalyst solution, then heating, filtering, washing, and drying to obtain a compound A;

[0007] In the above reaction process, p-chlorophenyltrimethoxysilane is hydrolyzed and polymerized to form a polyhedral structure, and KCl is fixed in the polyhedral structure in the form of a single nanoparticle.

[0008] Step (3) The intermediate and stannous chloride dihydrate are mixed uniformly, and then ethanol and 37 wt% concentrated hydrochloric acid are added, heated, reacted, and a yellow transparent solution is obtained; the pH is adjusted to 8 with a NaOH aqueous solution, allowed to stand, filtered, extracted, and compound B is obtained;

[0009] In the above reaction process, triphenylphosphine oxide introduces a meta-nitro group on the benzene ring under the action of a nitrating agent to obtain an intermediate; the nitro group in the intermediate is then converted into an amine group to obtain compound B.

[0010] Step (4) Mix the surface-modified PC resin, compound B, toluene and triethylamine, stir, add the dispersion of compound A dropwise at room temperature and nitrogen atmosphere, and heat to react.

[0011] After the reaction is completed, the flame retardant PC resin is obtained by purification and drying;

[0012] In the above reaction process, -Cl in compound A undergoes substitution reaction with the surface modified PC resin and the amine group in compound B to form a cross-linking system, and at the same time, compound A and compound B are connected to the surface of the PC resin to obtain a flame retardant PC resin.

[0013] Step (5) adding antioxidant, masterbatch, lubricant and hydrolysis resistance agent to the flame retardant PC resin, heating, heat preservation and fully mixing, then adding epoxy resin, thermoplastic polyurethane elastomer and gelatin, heating and then cooling to obtain a mixed system; injection molding the mixed system, demolding, and obtaining a flame retardant PC plastic.

[0014] Preferably, in the step (1), the volume fraction of ethylenediamine in the ethanol solution of ethylenediamine is 1.0-1.5%; the usage ratio of PC resin to the ethanol solution of ethylenediamine is 29-40kg:800-1200L; the heating temperature is 50-70°C; the soaking reaction time is 8-15min; the cooling time is 5-10min; the washing liquid used for washing is ethanol; and the drying method is air flow drying.

[0015] Preferably, in step (2), the heating temperature is 55-65°C; the reaction time is 1-1.5h; the heating condition is to heat to 65-75°C and maintain for 20-30h; the washing method is to wash the filter residue with ethanol and distilled water in turn, and repeat the washing 3-5 times; the drying condition is to vacuum dry at 110-130°C for 4-6h.

[0016] Preferably, in the step (2), the preparation method of the p-chlorophenyltrimethoxysilane dispersion is as follows: 11.6-23.2 kg of p-chlorophenyltrimethoxysilane is added to 100-200 L of acetone, and stirred at a speed of 150-300 r / min for 30-60 min; the preparation method of the KCl aqueous solution is as follows: 0.04-0.06 kg of KCl is dissolved in 1-2 L of distilled water and stirred until all the solids are dissolved; the preparation method of the catalyst solution is as follows: 0.075-0.15 kg of tetramethylammonium hydroxide is dissolved in 1.5-3 L of deionized water.

[0017] Preferably, in the step (3), the preparation method of the intermediate is as follows: 27.8-55.6 kg of triphenylphosphine oxide is dispersed in 400-800 L of 95-98% concentrated sulfuric acid at -5-0°C to obtain a triphenylphosphine oxide dispersion; 200-400 L of 95-98% concentrated sulfuric acid and 30-60 kg of 65-68% nitric acid are fully mixed and stirred at -5°C to obtain a nitrating agent; the nitrating agent is dripped into the triphenylphosphine oxide dispersion at -5-0°C, and after 1 hour of the completion of the dropwise addition, the mixture is brought to room temperature and reacted for 5-6 hours. After the reaction is completed, the reaction solution is poured into 300-600 kg of crushed ice cubes while stirring, and after the ice cubes are melted, the mixture is filtered by suction, and the filter cake is washed 3 times with distilled water and dried to obtain the intermediate.

[0018] Preferably, in the step (3), the usage ratio of the intermediate, stannous chloride dihydrate, ethanol and concentrated hydrochloric acid is 33-66kg:180-360kg:540-1100L:270-540L; the heating temperature is 33-40°C, and the reaction time is 4.5-5.5h; the NaOH aqueous solution adopts a 20-30wt% NaOH aqueous solution; and the extraction method is to extract the filtrate with chloroform 3-6 times.

[0019] Preferably, in the step (4), the dispersion of compound A is obtained by dispersing 15-30 kg of compound A in 50-100 L of toluene; the amount ratio of the surface modified PC resin, compound B, toluene and triethylamine is 7-14 kg: 3-6 kg: 25-50 L: 3.7-7.4 kg; stirring conditions: stirring at a speed of 150-300 r / min for 20-30 min; heating reaction conditions: raising the temperature to 75-85°C and maintaining the reaction for 11-14 h; purification method: after the reaction is completed, the triethylamine salt is filtered under reduced pressure, and the toluene is removed by rotary evaporation to obtain a crude product, which is then dissolved in dichloromethane and washed with deionized water for 3-5 times until the organic layer is neutral, and finally, the dichloromethane is removed by rotary evaporation; drying conditions: vacuum drying at 90-110°C for 20-30 h.

[0020] Preferably, in step (5), the dosage ratio of flame retardant PC resin, antioxidant, masterbatch, lubricant, hydrolysis resistance agent, epoxy resin, thermoplastic polyurethane elastomer and gelatin is: 10-16kg: 0.02-0.1kg: 0-0.8kg: 0.02-0.06kg: 0.06-0.12kg: 0.24-0.4kg: 0.04-0.3kg: 0.3-0.5kg; wherein the epoxy value of the epoxy resin is greater than 0.35.

[0021] Preferably, in step (5), the heating temperature is 255-260°C; the heating and cooling conditions are as follows: heating to 285-290°C, heating for 30-40s, and then cooling to 235-245°C; the injection molding conditions are as follows: the injection pressure is 70-150MPa, the mold temperature during injection is 140-170°C, the screw speed is 30-50rpm, and after the injection is completed, the mold temperature is cooled to 70-80°C at a rate of 5-8°C / min.

[0022] A flame retardant PC plastic prepared by adopting a method for preparing a flame retardant PC plastic.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. In the present invention, the PC resin is surface-modified, free amine groups are introduced into the PC resin surface in the form of chemical bonds, flame retardants are grafted onto the PC resin surface through the free amine groups, various additives are added, and flame-retardant PC plastics are obtained by injection molding. The flame retardant of the present invention is connected to the PC resin in the form of chemical bonds. Compared with the conventional PC plastic preparation process in which the flame retardant and the PC resin are directly blended and extruded, the problem of poor compatibility between the flame retardant and the PC resin is solved, and the flame retardant effect of the PC flame retardant plastic can be improved; at the same time, the adverse effects of the flame retardant on the transparency and light transmittance of the PC plastic are minimized.

[0025] 2. In the present invention, -Cl in compound A undergoes substitution reaction with the surface-modified PC resin and the amine group in compound B to form a cross-linking system, thereby improving the stability of the flame retardant system; further, the N, P, and Si flame retardant systems are introduced into the PC resin through the reaction, and the three work together to greatly improve the flame retardant properties of the flame retardant plastic.

[0026] 3. In the present invention, KCl nanocrystals are introduced into the polyhedral structure of compound B. The addition of KCl nanocrystals helps to improve the thermal stability of compound B, improve the quality of the carbon layer during the combustion process, effectively inhibit the effect of heat and mass transfer, and further enhance the flame retardant effect of PC flame retardant plastics. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a process flow chart of the preparation of the flame retardant PC plastic of the present invention;

[0028] Figure 2 It is a schematic diagram of the synthesis of compound B in the present invention;

[0029] Figure 3 It is a comparison chart of limiting oxygen index test of flame retardant PC plastics of Examples 1-5 and Comparative Examples 1-5 in the present invention. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] This embodiment discloses a method for preparing a flame retardant PC plastic, comprising the following steps:

[0033] Step (1) 29 kg of PC resin was added to 800 L of ethanol solution with a volume fraction of 1.0% ethylenediamine, heated to 50° C., and immersed in a sealed environment for reaction for 8 min. After the reaction was completed, it was cooled for 5 min, filtered, washed with ethanol, and dried with air flow to obtain a surface-modified PC resin.

[0034] Step (2) adding 11.6 kg of p-chlorophenyltrimethoxysilane to 100 L of acetone, stirring at a speed of 150 r / min for 30 min to obtain a p-chlorophenyltrimethoxysilane dispersion; dissolving 0.04 kg of KCl in 1 L of distilled water and stirring until the solid is completely dissolved to obtain a KCl aqueous solution; dissolving 0.075 kg of tetramethylammonium hydroxide in 1.5 L of deionized water to obtain a catalyst solution; mixing the p-chlorophenyltrimethoxysilane dispersion with the KCl aqueous solution, heating to 55° C., reacting for 1 h, then dropwise adding the catalyst solution, then heating to 65° C. and maintaining for 20 h, filtering, washing the filter residue with ethanol and distilled water in turn, repeating the washing 3 times, and vacuum drying at 110° C. for 4 h to obtain compound A.

[0035] Step (3) dispersing 27.8 kg of triphenylphosphine oxide in 400 L of 95% concentrated sulfuric acid at -5°C to obtain a triphenylphosphine oxide dispersion; fully mixing and stirring 200 L of 95% concentrated sulfuric acid and 30 kg of 65% nitric acid at -5°C to obtain a nitrating agent; dripping the nitrating agent into the triphenylphosphine oxide dispersion dropwise at -5°C, and after 1 hour of the completion of the dropwise addition, transferring the mixture to room temperature and reacting for 5 hours. After the reaction is completed, pouring the reaction solution into 300 kg of crushed ice cubes while stirring, and after the ice cubes are melted, filtering with suction, washing the filter cake with distilled water for 3 times, and drying to obtain an intermediate; uniformly mixing 33 kg of the intermediate with 180 kg of stannous chloride dihydrate, and then adding 540 L of ethanol, 270 L of ethanol, and 100 L of stannic chloride. 37wt% concentrated hydrochloric acid, heated to 33°C, reacted for 4.5h to obtain a yellow transparent solution; the pH of the yellow transparent solution was adjusted to 8 with 20wt% NaOH aqueous solution, allowed to stand, filtered, and the filtrate was extracted with chloroform for 3 times to obtain compound B.

[0036] Step (4) dispersing 15 kg of compound A in 50 L of toluene to obtain a dispersion of compound A; mixing 7 kg of surface modified PC resin, 3 kg of compound B, 25 L of toluene and 3.7 kg of triethylamine, stirring at a speed of 150 r / min for 20 min, adding the dispersion of compound A dropwise at room temperature and nitrogen atmosphere, raising the temperature to 75°C and maintaining the reaction for 11 h. After the reaction is completed, filtering the triethylamine salt under reduced pressure, removing toluene by rotary evaporation to obtain a crude product, then dissolving the crude product in dichloromethane, washing with deionized water 3 times until the organic layer is neutral, finally, removing dichloromethane by rotary evaporation, and vacuum drying at 90°C for 20 h to obtain a flame retardant PC resin.

[0037] Step (5) adding 0.02kg antioxidant, 0kg masterbatch, 0.02kg lubricant and 0.06kg anti-hydrolysis agent to 10kg flame-retardant PC resin, heating to 255°C, keeping warm and fully mixing for 60s, adding 0.24kg epoxy resin with an epoxy value greater than 0.35, 0.04kg thermoplastic polyurethane elastomer and 0.3kg gelatin, heating to 285°C, heating for 30s, cooling to 235°C to obtain a mixed system; injection molding the mixed system, the injection pressure is 70MPa, the mold temperature during injection is 140°C, the screw speed is 30rpm, after the injection is completed, the mold temperature is cooled to 70°C at a rate of 5°C / min, demolding, and obtaining a flame-retardant PC plastic.

[0038] Example 2

[0039] This embodiment discloses a method for preparing a flame retardant PC plastic, comprising the following steps:

[0040] Step (1) 40 kg of PC resin is added to 1200 L of ethanol solution with a volume fraction of 1.5% ethylenediamine, heated to 70° C., and immersed in a sealed environment for reaction for 15 min. After the reaction is completed, it is cooled for 10 min, filtered, washed with ethanol, and dried with air flow to obtain a surface-modified PC resin.

[0041] Step (2) adding 23.2 kg of p-chlorophenyltrimethoxysilane to 200 L of acetone, stirring at a speed of 300 r / min for 60 min to obtain a p-chlorophenyltrimethoxysilane dispersion; dissolving 0.06 kg of KCl in 2 L of distilled water and stirring until the solid is completely dissolved to obtain a KCl aqueous solution; dissolving 0.15 kg of tetramethylammonium hydroxide in 3 L of deionized water to obtain a catalyst solution; mixing the p-chlorophenyltrimethoxysilane dispersion with the KCl aqueous solution, heating to 65° C., reacting for 1.5 h, then dripping the catalyst solution, then heating to 75° C. and maintaining for 30 h, filtering, washing the filter residue with ethanol and distilled water in turn, repeating the washing 5 times, and vacuum drying at 130° C. for 6 h to obtain compound A.

[0042] Step (3) dispersing 55.6 kg of triphenylphosphine oxide in 800 L of 98% concentrated sulfuric acid at 0° C. to obtain a triphenylphosphine oxide dispersion; fully mixing and stirring 400 L of 98% concentrated sulfuric acid and 60 kg of 68% nitric acid at -5° C. to obtain a nitrating agent; dripping the nitrating agent dropwise into the triphenylphosphine oxide dispersion at 0° C., 1 hour after the dropwise addition is completed, moving to room temperature, reacting for 6 hours, and after the reaction is completed, pouring the reaction solution into 600 kg of crushed ice cubes while stirring, and after the ice cubes are melted, filtering with suction, washing the filter cake with distilled water for 3 times, and drying to obtain an intermediate; mixing 66 kg of the intermediate with 360 kg of stannous chloride dihydrate, and then adding 1100 L of ethanol and 540 L of ethanol. 37wt% concentrated hydrochloric acid, heated to 40°C, reacted for 5.5h to obtain a yellow transparent solution; the pH of the yellow transparent solution was adjusted to 8 with 30wt% NaOH aqueous solution, allowed to stand, filtered, and the filtrate was extracted with chloroform for 6 times to obtain compound B.

[0043] Step (4) dispersing 30 kg of compound A in 100 L of toluene to obtain a dispersion of compound A; mixing 14 kg of surface modified PC resin, 6 kg of compound B, 50 L of toluene and 7.4 kg of triethylamine, stirring at a speed of 300 r / min for 30 min, adding the dispersion of compound A dropwise at room temperature and nitrogen atmosphere, raising the temperature to 85° C. and maintaining the reaction for 14 h. After the reaction is completed, filtering the triethylamine salt under reduced pressure, removing toluene by rotary evaporation to obtain a crude product, then dissolving the crude product in dichloromethane, washing with deionized water 5 times until the organic layer is neutral, finally, removing dichloromethane by rotary evaporation, and vacuum drying at 110° C. for 30 h to obtain a flame retardant PC resin.

[0044] Step (5) adding 0.1 kg antioxidant, 0.8 kg masterbatch, 0.06 kg lubricant and 0.12 kg anti-hydrolysis agent to 16 kg flame-retardant PC resin, heating to 260° C., keeping warm and fully mixing for 90 seconds, adding 0.4 kg epoxy resin with an epoxy value greater than 0.35, 0.3 kg thermoplastic polyurethane elastomer and 0.5 kg gelatin, heating to 290° C., heating for 40 seconds, and then cooling to 245° C. to obtain a mixed system; injection molding the mixed system, the injection pressure is 150 MPa, the mold temperature during injection is 170° C., the screw speed is 50 rpm, after the injection is completed, the mold temperature is cooled to 80° C. at a rate of 8° C. / min, demolding, and obtaining a flame-retardant PC plastic.

[0045] Example 3

[0046] This embodiment discloses a method for preparing a flame retardant PC plastic, comprising the following steps:

[0047] Step (1) 35 kg of PC resin is added to 1000 L of ethanol solution with a volume fraction of 1.2% ethylenediamine, heated to 60° C., and immersed in a sealed environment for reaction for 12 min. After the reaction is completed, it is cooled for 8 min, filtered, washed with ethanol, and dried with air flow to obtain a surface-modified PC resin.

[0048] Step (2) adding 18.0 kg of p-chlorophenyltrimethoxysilane to 150 L of acetone, stirring at a speed of 220 r / min for 50 min to obtain a p-chlorophenyltrimethoxysilane dispersion; dissolving 0.05 kg of KCl in 1.5 L of distilled water and stirring until the solid is completely dissolved to obtain a KCl aqueous solution; dissolving 0.11 kg of tetramethylammonium hydroxide in 2.5 L of deionized water to obtain a catalyst solution; mixing the p-chlorophenyltrimethoxysilane dispersion with the KCl aqueous solution, heating to 60° C., reacting for 1.2 h, then dripping the catalyst solution, then heating to 70° C. and maintaining for 25 h, filtering, washing the filter residue with ethanol and distilled water in turn, repeating the washing 4 times, and vacuum drying at 120° C. for 5 h to obtain compound A.

[0049] Step (3) dispersing 40.6 kg of triphenylphosphine oxide in 600 L of 97% concentrated sulfuric acid at -3°C to obtain a triphenylphosphine oxide dispersion; fully mixing and stirring 300 L of 97% concentrated sulfuric acid and 40 kg of 67% nitric acid at -5°C to obtain a nitrating agent; dripping the nitrating agent into the triphenylphosphine oxide dispersion dropwise at -3°C, and after 1 hour of the completion of the dropwise addition, transferring the mixture to room temperature and reacting for 5.5 hours. After the reaction is completed, pouring the reaction solution into 400 kg of crushed ice cubes while stirring, and after the ice cubes are melted, filtering with suction, washing the filter cake with distilled water for 3 times, and drying to obtain an intermediate; uniformly mixing 46 kg of the intermediate with 280 kg of stannous chloride dihydrate, and then adding 750 L of ethanol, 390 L of ethanol, and 100 L of stannic chloride. 37wt% concentrated hydrochloric acid, heated to 37°C, reacted for 5.0h to obtain a yellow transparent solution; the pH of the yellow transparent solution was adjusted to 8 with 25wt% NaOH aqueous solution, allowed to stand, filtered, and the filtrate was extracted with chloroform for 4 times to obtain compound B.

[0050] Step (4) dispersing 22 kg of compound A in 70 L of toluene to obtain a dispersion of compound A; mixing 10 kg of surface modified PC resin, 4.5 kg of compound B, 35 L of toluene, and 5.7 kg of triethylamine, stirring at a speed of 250 r / min for 25 min, adding the dispersion of compound A dropwise at room temperature and a nitrogen atmosphere, raising the temperature to 80° C. and maintaining the reaction for 13 h. After the reaction is completed, filtering the triethylamine salt under reduced pressure, removing toluene by rotary evaporation to obtain a crude product, then dissolving the crude product in dichloromethane, washing with deionized water 4 times until the organic layer is neutral, finally, removing dichloromethane by rotary evaporation, and vacuum drying at 100° C. for 25 h to obtain a flame retardant PC resin.

[0051] Step (5) adding 0.06 kg antioxidant, 0.4 kg masterbatch, 0.04 kg lubricant and 0.08 kg anti-hydrolysis agent to 12 kg flame retardant PC resin, heating to 257 ° C, keeping warm and fully mixing for 70 seconds, adding 0.32 kg epoxy resin with an epoxy value greater than 0.35, 0.2 kg thermoplastic polyurethane elastomer, and 0.4 kg gelatin, heating to 287 ° C, heating for 35 seconds, and then cooling to 240 ° C to obtain a mixed system; injection molding the mixed system, the injection pressure is 110 MPa, the mold temperature during injection is 150 ° C, the screw speed is 40 rpm, after the injection is completed, the mold temperature is cooled to 75 ° C at a rate of 6 ° C / min, demolding, and obtaining a flame retardant PC plastic.

[0052] Example 4

[0053] This embodiment discloses a method for preparing a flame retardant PC plastic, comprising the following steps:

[0054] Step (1) 32 kg of PC resin is added to 900 L of ethanol solution with a volume fraction of 1.1% ethylenediamine, heated to 55° C., and immersed in a sealed environment for reaction for 10 min. After the reaction is completed, it is cooled for 6 min, filtered, washed with ethanol, and dried with air flow to obtain a surface-modified PC resin.

[0055] Step (2) adding 15.6 kg of p-chlorophenyltrimethoxysilane to 120 L of acetone, stirring at a speed of 200 r / min for 40 min to obtain a p-chlorophenyltrimethoxysilane dispersion; dissolving 0.045 kg of KCl in 1.2 L of distilled water and stirring until the solid is completely dissolved to obtain a KCl aqueous solution; dissolving 0.09 kg of tetramethylammonium hydroxide in 2.0 L of deionized water to obtain a catalyst solution; mixing the p-chlorophenyltrimethoxysilane dispersion with the KCl aqueous solution, heating to 58° C., reacting for 1.1 h, then dripping the catalyst solution, then heating to 68° C. and maintaining for 23 h, filtering, washing the filter residue with ethanol and distilled water in turn, repeating the washing 3 times, and vacuum drying at 115° C. for 4.5 h to obtain compound A.

[0056] Step (3) dispersing 35.6 kg of triphenylphosphine oxide in 500 L of 96% concentrated sulfuric acid at -4°C to obtain a triphenylphosphine oxide dispersion; fully mixing and stirring 250 L of 96% concentrated sulfuric acid and 35 kg of 66% nitric acid at -5°C to obtain a nitrating agent; dripping the nitrating agent into the triphenylphosphine oxide dispersion dropwise at -4°C, and after 1 hour of the completion of the dropwise addition, transferring the mixture to room temperature and reacting for 5.2 hours. After the reaction is completed, pouring the reaction mixture into 350 kg of crushed ice cubes while stirring, and after the ice cubes are melted, filtering with suction, washing the filter cake with distilled water for 3 times, and drying to obtain an intermediate; uniformly mixing 40 kg of the intermediate with 240 kg of stannous chloride dihydrate, and then adding 650 L of ethanol and 330 L of ethanol. 37wt% concentrated hydrochloric acid, heated to 35°C, reacted for 4.8h to obtain a yellow transparent solution; the pH of the yellow transparent solution was adjusted to 8 with 23wt% NaOH aqueous solution, allowed to stand, filtered, and the filtrate was extracted with chloroform three times to obtain compound B.

[0057] Step (4) dispersing 18 kg of compound A in 60 L of toluene to obtain a dispersion of compound A; mixing 8 kg of surface modified PC resin, 4 kg of compound B, 30 L of toluene and 4.7 kg of triethylamine, stirring at a speed of 200 r / min for 23 min, adding the dispersion of compound A dropwise at room temperature and nitrogen atmosphere, raising the temperature to 78° C. and maintaining the reaction for 12 h. After the reaction is completed, filtering the triethylamine salt under reduced pressure, removing toluene by rotary evaporation to obtain a crude product, then dissolving the crude product in dichloromethane, washing with deionized water three times until the organic layer is neutral, finally, removing dichloromethane by rotary evaporation, and vacuum drying at 95° C. for 23 h to obtain a flame retardant PC resin.

[0058] Step (5) adding 0.04kg antioxidant, 0.2kg masterbatch, 0.03kg lubricant and 0.07kg anti-hydrolysis agent to 11kg flame-retardant PC resin, heating to 256°C, keeping warm and fully mixing for 65s, adding 0.28kg epoxy resin with an epoxy value greater than 0.35, 0.1kg thermoplastic polyurethane elastomer, and 0.35kg gelatin, heating to 286°C, heating for 33s, and then cooling to 238°C to obtain a mixed system; injection molding the mixed system, the injection pressure is 90MPa, the mold temperature during injection is 145°C, the screw speed is 35rpm, after the injection is completed, the mold temperature is cooled to 72°C at a rate of 6°C / min, demolding, and obtaining a flame-retardant PC plastic.

[0059] Example 5

[0060] This embodiment discloses a method for preparing a flame retardant PC plastic, comprising the following steps:

[0061] Step (1) 38 kg of PC resin was added to 1100 L of ethanol solution with a volume fraction of 1.3% ethylenediamine, heated to 65, immersed in a sealed environment for reaction for 14 min, cooled for 8 min after the reaction was completed, filtered, washed with ethanol, and dried with air flow to obtain a surface-modified PC resin.

[0062] Step (2) adding 20.5 kg of p-chlorophenyltrimethoxysilane to 180 L of acetone, stirring at a speed of 250 r / min for 55 min to obtain a p-chlorophenyltrimethoxysilane dispersion; dissolving 0.055 kg of KCl in 1.8 L of distilled water and stirring until the solid is completely dissolved to obtain a KCl aqueous solution; dissolving 0.13 kg of tetramethylammonium hydroxide in 2.8 L of deionized water to obtain a catalyst solution; mixing the p-chlorophenyltrimethoxysilane dispersion with the KCl aqueous solution, heating to 62° C., reacting for 1.4 h, then dripping the catalyst solution, then heating to 72° C. and maintaining for 28 h, filtering, washing the filter residue with ethanol and distilled water in turn, repeating the washing 4 times, and vacuum drying at 110-130° C. for 5.5 h to obtain compound A.

[0063] Step (3) dispersing 45.6 kg of triphenylphosphine oxide in 700 L of 97% concentrated sulfuric acid at -2°C to obtain a triphenylphosphine oxide dispersion; fully mixing and stirring 350 L of 97% concentrated sulfuric acid and 50 kg of 67% nitric acid at -5°C to obtain a nitrating agent; dripping the nitrating agent into the triphenylphosphine oxide dispersion dropwise at -2°C, and after 1 hour of the completion of the dropwise addition, transferring the mixture to room temperature and reacting for 5.8 hours. After the reaction is completed, pouring the reaction solution into 500 kg of crushed ice cubes while stirring, and after the ice cubes are melted, filtering with suction, washing the filter cake with distilled water for 3 times, and drying to obtain an intermediate; mixing 56 kg of the intermediate with 320 kg of stannous chloride dihydrate, and then adding 900 L of ethanol, 460 L of ethanol, and 100 L of stannic chloride. 37wt% concentrated hydrochloric acid, heated to 39°C, reacted for 5.2h to obtain a yellow transparent solution; the pH of the yellow transparent solution was adjusted to 8 with 28wt% NaOH aqueous solution, allowed to stand, filtered, and the filtrate was extracted with chloroform for 5 times to obtain compound B.

[0064] Step (4) dispersing 26 kg of compound A in 85 L of toluene to obtain a dispersion of compound A; mixing 12 kg of surface modified PC resin, 5 kg of compound B, 40 L of toluene, and 6.3 kg of triethylamine, stirring at a speed of 280 r / min for 25 min, adding the dispersion of compound A dropwise at room temperature and a nitrogen atmosphere, raising the temperature to 83° C. and maintaining the reaction for 13 h. After the reaction is completed, filtering the triethylamine salt under reduced pressure, removing toluene by rotary evaporation to obtain a crude product, then dissolving the crude product in dichloromethane, washing with deionized water 5 times until the organic layer is neutral, finally, removing dichloromethane by rotary evaporation, and vacuum drying at 105° C. for 28 h to obtain a flame retardant PC resin.

[0065] Step (5) adding 0.08 kg antioxidant, 0.6 kg masterbatch, 0.05 kg lubricant and 0.1 kg anti-hydrolysis agent to 14 kg flame retardant PC resin, heating to 258 ° C, keeping warm and fully mixing for 80 seconds, adding 0.36 kg epoxy resin with an epoxy value greater than 0.35, 0.25 kg thermoplastic polyurethane elastomer, and 0.45 kg gelatin, heating to 289 ° C, heating for 38 seconds, and then cooling to 242 ° C to obtain a mixed system; injection molding the mixed system, the injection pressure is 130 MPa, the mold temperature during injection is 160 ° C, the screw speed is 45 rpm, after the injection is completed, the mold temperature is cooled to 78 ° C at a rate of 7 ° C / min, demolding, and flame retardant PC plastic is obtained.

[0066] Comparative Example 1

[0067] Comparative Example 1 Compared with Example 4, in the process of preparing the flame-retardant PC resin, compound A was not added, and other conditions remained unchanged.

[0068] Comparative Example 2

[0069] Comparative Example 2 Compared with Example 4, in the process of preparing the flame retardant PC resin, compound B was not added, and other conditions remained unchanged.

[0070] Comparative Example 3

[0071] Comparative Example 3 Compared with Example 4, in the process of preparing the flame-retardant PC resin, PC resin was used instead of the surface-modified PC resin, and other conditions remained unchanged.

[0072] Comparative Example 4

[0073] Comparative Example 4 Compared with Example 4, during the preparation of Compound A, no KCl aqueous solution was added, and other conditions remained unchanged.

[0074] Experimental example

[0075] The flame retardant PC plastics in Examples 1-5 and Comparative Examples 1-4 were tested for performance:

[0076] Test 1. Limiting oxygen index test: The test was conducted according to ASTM D2863, and the sample size was: 120mm×10mm×4mm.

[0077] Test 2: Vertical burning test: The vertical burning method (UL 94) is to apply flame to a vertically placed sample. According to the degree of combustion of the material, it is divided into three grades: V-0, V-1 and V-2. The test is carried out in accordance with ASTM D3801-2010 standard. The sample size is: 130mm×13mm×3.2mm.

[0078] The test results are shown in Table 1:

[0079] Table 1

[0080]

[0081]

[0082] It can be seen from the test results in Table 1 that the flame retardant PC plastics prepared in Examples 1-5 of the present invention have excellent flame retardant effects, the limiting oxygen index can reach up to 36.3%, and there is no dripping phenomenon during the combustion process.

[0083] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing flame retardant PC plastics, It is characterized in that The following steps are involved: Step (1) adding PC resin to an ethanol solution of ethylenediamine, heating, soaking and reacting in a sealed environment, cooling, filtering, washing, and drying to obtain a surface-modified PC resin; Step (2) mixing a p-chlorophenyltrimethoxysilane dispersion with a KCl aqueous solution, heating, reacting, then dropping a catalyst solution, then heating, filtering, washing, and drying to obtain a compound A; Step (3) The intermediate and stannous chloride dihydrate are mixed uniformly, and then ethanol and 37 wt% concentrated hydrochloric acid are added, heated, and reacted to obtain a yellow transparent solution; the pH is adjusted to 8 with a NaOH aqueous solution, and the mixture is allowed to stand, filtered, and extracted to obtain compound B; Step (4) mixing the surface-modified PC resin, compound B, toluene and triethylamine, stirring, adding dropwise the dispersion of compound A at room temperature and in a nitrogen atmosphere, heating the mixture for reaction, purifying and drying the mixture after the reaction is completed to obtain a flame-retardant PC resin; Step (5) adding antioxidant, masterbatch, lubricant and hydrolysis resistance agent to the flame retardant PC resin, heating, heat preservation and fully mixing, then adding epoxy resin, thermoplastic polyurethane elastomer and gelatin, heating and then cooling to obtain a mixed system; injection molding the mixed system, demolding, and obtaining a flame retardant PC plastic.

2. The method for preparing the flame retardant PC plastic according to claim 1, It is characterized in that In the step (1), the volume fraction of ethylenediamine in the ethanol solution of ethylenediamine is 1.0-1.5%; the usage ratio of PC resin to the ethanol solution of ethylenediamine is 29-40kg:800-1200L; the heating temperature is 50-70°C; the soaking reaction time is 8-15min; the cooling time is 5-10min; the washing liquid used for washing is ethanol; and the drying method is air flow drying.

3. The method for preparing the flame retardant PC plastic according to claim 1, It is characterized in that In the step (2), the heating temperature is 55-65°C; the reaction time is 1-1.5h; the heating condition is to heat to 65-75°C and maintain for 20-30h; the washing method is to wash the filter residue with ethanol and distilled water in turn, and repeat the washing 3-5 times; the drying condition is to vacuum dry at 110-130°C for 4-6h.

4. The method for preparing the flame retardant PC plastic according to claim 1, It is characterized in that In the step (2), the preparation method of the p-chlorophenyltrimethoxysilane dispersion is as follows: 11.6-23.2 kg of p-chlorophenyltrimethoxysilane is added to 100-200 L of acetone, and stirred at a speed of 150-300 r / min for 30-60 min; the preparation method of the KCl aqueous solution is as follows: 0.04-0.06 kg of KCl is dissolved in 1-2 L of distilled water and stirred until all the solids are dissolved; the preparation method of the catalyst solution is as follows: 0.075-0.15 kg of tetramethylammonium hydroxide is dissolved in 1.5-3 L of deionized water.

5. The method for preparing the flame retardant PC plastic according to claim 1, It is characterized in that In the step (3), the preparation method of the intermediate is as follows: 27.8-55.6 kg of triphenylphosphine oxide is dispersed in 400-800 L of 95-98% concentrated sulfuric acid at -5-0°C to obtain a triphenylphosphine oxide dispersion; 200-400 L of 95-98% concentrated sulfuric acid and 30-60 kg of 65-68% nitric acid are fully mixed and stirred at -5°C to obtain a nitrating agent; the nitrating agent is dripped into the triphenylphosphine oxide dispersion at -5-0°C, and after 1 hour of the completion of the dripping, the mixture is moved to room temperature and reacted for 5-6 hours. After the reaction is completed, the reaction solution is poured into 300-600 kg of crushed ice cubes while stirring, and after the ice cubes are melted, the mixture is filtered by suction, and the filter cake is washed 3 times with distilled water and dried to obtain the intermediate.

6. The method for preparing the flame retardant PC plastic according to claim 1, It is characterized in that In the step (3), the usage ratio of the intermediate, stannous chloride dihydrate, ethanol and concentrated hydrochloric acid is 33-66kg:180-360kg:540-1100L:270-540L; the heating temperature is 33-40°C, and the reaction time is 4.5-5.5h; the NaOH aqueous solution adopts a 20-30wt% NaOH aqueous solution; and the extraction method is to extract the filtrate with chloroform for 3-6 times.

7. The method for preparing the flame retardant PC plastic according to claim 1, It is characterized in that In the step (4), the dispersion of compound A is obtained by dispersing 15-30 kg of compound A in 50-100 L of toluene; The dosage ratio of surface modified PC resin, compound B, toluene and triethylamine is 7-14kg:3-6kg:25-50L:3.7-7.4kg; stirring conditions: stirring at a speed of 150-300r / min for 20-30min; heating reaction conditions: raising the temperature to 75-85°C and maintaining the reaction for 11-14h; purification method: after the reaction is completed, the triethylamine salt is filtered under reduced pressure, and the toluene is removed by rotary evaporation to obtain a crude product, and then the crude product is dissolved in dichloromethane, washed with deionized water for 3-5 times until the organic layer is neutral, and finally, the dichloromethane is removed by rotary evaporation; drying conditions: vacuum drying at 90-110°C for 20-30h.

8. The method for preparing the flame retardant PC plastic according to claim 1, It is characterized in that In the step (5), the usage ratio of flame retardant PC resin, antioxidant, masterbatch, lubricant, hydrolysis resistance agent, epoxy resin, thermoplastic polyurethane elastomer and gelatin is 10-16kg: 0.02-0.1kg: 0-0.8kg: 0.02-0.06kg: 0.06-0.12kg: 0.24-0.4kg: 0.04-0.3kg: 0.3-0.5kg; wherein the epoxy value of the epoxy resin is greater than 0.

35.

9. The method for preparing the flame retardant PC plastic according to claim 1, It is characterized in that In the step (5), the heating temperature is 255-260°C; the heating and cooling conditions are as follows: heating to 285-290°C, heating for 30-40s, and then cooling to 235-245°C; the injection molding conditions are as follows: the injection pressure is 70-150MPa, the mold temperature during injection is 140-170°C, the screw speed is 30-50rpm, and after the injection is completed, the mold temperature is cooled to 70-80°C at a rate of 5-8°C / min.

10. A flame retardant PC plastic prepared by the method according to any one of claims 1 to 9.