Low-temperature-resistant and aging-resistant modified polycarbonate composition and preparation method thereof
By mixing polycarbonate with polysiloxane-polycarbonate random copolymer and nanoTiO2 in proportion, a modified polycarbonate composition that is resistant to low temperature and aging is prepared, and the aging of polycarbonate materials is solved. Problem, improving mechanical properties and flame retardant properties, suitable for high-demand places.
Patent Information
- Application Number
- CN202411266410.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
AI Technical Summary
Polycarbonate materials are prone to aging under low temperature and light, resulting in structural changes and degradation of performance, especially reduced mechanical properties and heat resistance, and there are problems of thermal aging and photoaging.
Polycarbonate, polysiloxane-polycarbonate random copolymer, nanoTiO2, compatibility agent, lubricant and ultraviolet absorber are mixed in a specific proportion, and melt-molded through a twin-screw extruder to prepare low temperature resistance and resistance. Aged modified polycarbonate composition.
It improves the mechanical properties and aging resistance of polycarbonate materials, enhances flame retardant properties, and is simple in preparation process, and is suitable for places with high requirements for low temperature and aging resistance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high molecular polymers, and particularly relates to a low temperature resistant and aging resistant modified polycarbonate composition and a preparation method thereof. Background Art
[0002] Polycarbonate (PC for short) is an important engineering plastic with the characteristics of high strength, high toughness, good transparency, etc. It has excellent physical properties, chemical stability and heat resistance and is widely used in electrical appliances, optics, medical, sporting goods and other fields. However, with the increase of use time, polycarbonate materials will age and produce a series of aging products, which will have an adverse effect on the performance and service life of the material. The aging of polycarbonate materials is mainly divided into two types: thermal aging and light aging. Thermal aging refers to the aging phenomenon caused by long-term exposure of materials to high temperature environments, while light aging refers to the aging process of materials under sunlight or ultraviolet rays. Both aging methods will cause structural changes in polycarbonate materials, resulting in a decrease in performance. During the thermal aging process, the molecular chains of polycarbonate materials undergo reactions such as breaking, cross-linking or chain depolymerization, producing a large number of low molecular weight compounds. These low molecular weight compounds will evaporate from the material, causing the material to become brittle, yellow or even crack. In addition, it will also cause the mechanical properties of polycarbonate materials to deteriorate, such as reduced strength, toughness and heat resistance. Light aging is another important cause of polycarbonate material aging. The energy in sunlight or ultraviolet rays will be absorbed by polycarbonate materials, resulting in the breakage of molecular chains and changes in structure. These changes can cause problems such as yellowing, brittleness and decreased mechanical properties of the material. In addition, light aging can also cause the surface of polycarbonate materials to become rough, further affecting its appearance and service life. Summary of the invention
[0003] The present invention aims to avoid the deficiencies of the prior art and applications, and provides a low-temperature resistant and aging resistant modified polycarbonate composition and a preparation method thereof.
[0004] To achieve the above object, the technical solution adopted by the present invention is: a low temperature resistant and aging resistant modified polycarbonate composition and a preparation method thereof, characterized in that the polycarbonate composition is prepared by mixing the following components in parts by weight: Polycarbonate 70-76 parts; Polysiloxane-polycarbonate random copolymer 16-24 parts; Nano-TiO 2 2-4 parts; compatibilizer 3-5 parts; lubricant 0.1-0.5 parts; ultraviolet absorber 0.5-1 parts; The specific preparation method is as follows: polycarbonate is placed in silo 1, and polysiloxane-polycarbonate random copolymer, TiO 2, compatibilizer, lubricant, and ultraviolet absorber are mixed evenly and placed in silo 2; the materials in silo 1 and silo 2 are uniformly fed into the twin-screw extruder through a metering scale according to the proportion, and after melt extrusion molding, they are cooled, blown dry, and granulated, and the performance is analyzed and packaged.
[0005] Furthermore, the melt flow rate of the polycarbonate is 10-15 g / (10 min).
[0006] The weight of the polysiloxane block in the polysiloxane-polycarbonate random copolymer accounts for 18-22% of the total weight of the copolymer, and the melt flow rate is 0-5 g / (10 min).
[0007] The compatibilizer is SAN; the lubricant is zinc stearate; and the ultraviolet absorber is UV-P.
[0008] The melt extrusion process conditions of the twin-screw extruder are as follows: first stage temperature 220-240°C, second stage temperature 240-260°C, third stage temperature 260-265°C, die head temperature 245°C, residence time 1-2min, and die head pressure 2-4 MPa.
[0009] The invention has the advantages that the preparation process is simple, polysiloxane polycarbonate and nano-TiO 2 , improving the mechanical properties and aging resistance of PC, and also improving the flame retardant properties of the product, to obtain a low-temperature resistant, aging-resistant and uniform quality polycarbonate composition, which can be widely used in various places with high requirements for low-temperature and aging-resistant materials. DETAILED DESCRIPTION
[0010] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0011] Example 1 A low temperature resistant and aging resistant modified polycarbonate composition is prepared by mixing the following components in proportion: polycarbonate: Lotte PC1010, melt flow rate 12 g / (10min); Polysiloxane-polycarbonate random copolymer: Gansu Yinguang Polysilver Chemical Co., Ltd., melt flow rate 5 g / (10min), weight of polysiloxane block 20%; nano-TiO 2 ; Compatibilizer: SAN; Lubricant: zinc stearate; UV absorber: UV-P.
[0012] The mass fractions of the above components are shown in Table (I); The preparation method is as follows: Add polysiloxane-polycarbonate random copolymer, TiO 2, compatibilizer, toughening agent and UV absorber, mix well and place the materials in silo 2; place polycarbonate in silo 1, and let the materials in silo 1 and silo 2 enter the twin-screw extruder at a uniform speed through a metering scale according to the proportion, and after extrusion molding, cool and blow dry, granulate, analyze the performance and package.
[0013] The melt extrusion process conditions of the twin-screw extruder are: first stage temperature 220-240℃, second stage temperature 240-260℃, third stage temperature 260-265℃, die head temperature 245℃, residence time 1-2min, die head pressure 2-4 MPa. See Table (II) for test data.
[0014] Test method: Humidity and heat aging test: aging for 1000h at 85% humidity and 85℃ temperature.
[0015] UV aging: at an irradiance of 0.75W / (m 2 ٠ nm) for 1000 h.
[0016] Embodiment 2-5 The components of the modified polycarbonate composition are the same as those in Example 1, and the component ratios are shown in Table (I); the preparation method is the same as that in Example 1; and the test data are shown in Table (II).
[0017] Table (I) Table 2 According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs may also make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the invention should also fall within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A low temperature resistant and aging resistant modified polycarbonate composition and a preparation method thereof, It is characterized in that The polycarbonate composition is prepared by mixing the following components in parts by weight: Polycarbonate 70-76 parts; Polysiloxane-polycarbonate random copolymer 16-24 parts; Nano-TiO 2 2-4 parts; compatibilizer 3-5 parts; lubricant 0.1-0.5 parts; ultraviolet absorber 0.5-1 parts; The specific preparation method is as follows: polycarbonate is placed in silo 1, and polysiloxane-polycarbonate random copolymer, TiO 2 , compatibilizer, lubricant, and ultraviolet absorber are mixed evenly and placed in silo 2; the materials in silo 1 and silo 2 are uniformly fed into the twin-screw extruder through a metering scale according to the proportion, and after melt extrusion molding, they are cooled, blown dry, and granulated, and the performance is analyzed and packaged.
2. A low temperature resistant and aging resistant modified polycarbonate composition and a preparation method thereof as claimed in claim 1, Features: The melt flow rate of the polycarbonate is 10-15 g / (10 min).
3. A low temperature resistant and aging resistant modified polycarbonate composition and a preparation method thereof according to claim 1, Features: The weight of the polysiloxane block in the polysiloxane-polycarbonate random copolymer accounts for 18-22% of the total weight of the copolymer, and the melt flow rate is 0-5 g / (10min).
4. A low temperature resistant and aging resistant modified polycarbonate composition and a preparation method thereof as claimed in claim 1, Features: The compatibilizer is SAN; the lubricant is zinc stearate; and the ultraviolet absorber is UV-P.
5. A low temperature resistant and aging resistant modified polycarbonate composition and a preparation method thereof according to claim 1, Features: The melt extrusion process conditions of the twin-screw extruder are as follows: first stage temperature 220-240°C, second stage temperature 240-260°C, third stage temperature 260-265°C, die head temperature 245°C, residence time 1-2min, and die head pressure 2-4 MPa.