Solid-liquid phase change composite material and preparation method thereof
By reacting and induced phase separation in polyols by thermosetting resin and polyamine, a solid-liquid phase transformation composite material with high loading rate and no leakage was prepared, solving the problems of leakage and high energy consumption in the prior art, and achieving high efficiency, Environmentally friendly energy reuse.
Patent Information
- Application Number
- CN202411347294.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
AI Technical Summary
The leakage problems of existing solid-liquid phase change materials and the high energy consumption, high cost and low loading rate caused by high temperature and high pressure processes limit their application in the fields of building energy conservation and heat recovery.
By reacting and induced phase separation in the polyol by thermosetting resin and polyamine, a solid-liquid phase transformation composite material with high loading rate and no leakage was prepared. A simple and efficient process was adopted to avoid the use of chemical solvents.
It realizes the high loading rate (more than 94.5%) and long-life phase transformation characteristics of solid-liquid phase transformation composite materials. It has a simple process, energy-saving and environmentally friendly, and is suitable for energy reuse technology.
Smart Images

Figure CN118931154A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional composite materials, and in particular relates to a solid-liquid phase change composite material and a preparation method thereof. Background Art
[0002] The use of phase change materials' thermal storage properties has always been considered a key energy recycling technology. Phase change materials can absorb and release latent heat at a certain temperature, which can significantly improve the efficiency of energy utilization systems. Latent heat storage has been shown to have good application potential in the fields of building energy conservation, heat recovery, temperature control, etc. Organic solid-liquid phase change materials have large latent heat, wide phase change temperature range, and a wide variety of raw materials, and have greater practical application potential. However, the leakage problem of solid-liquid phase change materials limits their further practical application. At the same time, the existing preparation methods developed for this purpose, such as porous medium encapsulation, microencapsulation, introduction of cross-linked carrier materials, etc., usually use high temperature and high pressure processes, use chemical solvents, etc., which are complex processes, high energy consumption, and high costs, which do not conform to the current energy-saving and environmental protection concepts advocated; and the loading rate of the phase change composite material prepared in this way is less than 70%, resulting in a significant decrease in its latent heat compared to the bulk phase change material. Therefore, it is necessary to develop a non-leaking solid-liquid phase change composite material with a simple preparation process, environmental protection, low cost, and high loading rate. Summary of the invention
[0003] In order to solve at least one technical problem in the prior art, a solid-liquid phase change composite material and a preparation method thereof are provided. The solid-liquid phase change composite material has a high loading rate and no leakage, and the preparation process is simple, efficient, energy-saving and environmentally friendly. In order to achieve the above technical objectives, the technical solution adopted in the embodiment of the present invention is:
[0004] In a first aspect, an embodiment of the present invention provides a solid-liquid phase change composite material, wherein the solid-liquid phase change composite material is prepared by inducing phase separation through reaction of a thermosetting resin and a polyamine in a polyol.
[0005] Further, the polyol includes a polyether polyol;
[0006] The general formula of the polyether polyol is H-(OC4H8)n-OH, where n≥3.
[0007] Further, the thermosetting resin includes epoxy resin;
[0008] The epoxy resin includes a bisphenol epoxy resin;
[0009] The bisphenol epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AD epoxy resin, bisphenol S epoxy resin, hydroxymethyl bisphenol A epoxy resin, and resorcinol epoxy resin;
[0010] Further, the polyamine includes aliphatic polyamine;
[0011] The general formula of the aliphatic polyamine is H2N(-C n H 2n )x-(NH)y-NH2,n≥2,x≥1,y≥0,
[0012] The aliphatic polyamine includes at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine, ethylenediamine, and 1,6-hexanediamine;
[0013] Furthermore, calculated by weight, the solid-liquid phase change composite material comprises:
[0014] 100 parts of polyether polyol;
[0015] X parts of bisphenol epoxy resin, 5≤X≤20;
[0016] Y parts of aliphatic polyamine, Y = W*0.01*X,
[0017] Wherein, W=EM / n·a, W is the weight percentage of the aliphatic polyamine used in 100 parts of the bisphenol-type epoxy resin, E is the epoxy value of the bisphenol-type epoxy resin, M is the molecular weight of the aliphatic polyamine, n is the number of active hydrogen atoms of the aliphatic polyamine, and a is the purity (%) of the aliphatic polyamine.
[0018] In a second aspect, an embodiment of the present invention further provides a method for preparing a solid-liquid phase change composite material, using the above-mentioned solid-liquid phase change composite material, comprising the following steps:
[0019] Step a, preparing a liquid mixture of polyether polyol / bisphenol epoxy resin: by weight, putting 100 parts of solid polyether polyol and X parts (5≤X≤20) of bisphenol epoxy resin into a mixing kettle, setting the stirring rate of the mixing kettle to a first stirring rate, and heating the mixture to a preset temperature T0 so that the mixture is a transparent and uniform liquid, to obtain a liquid mixture of polyether polyol / bisphenol epoxy resin, and keeping the liquid mixture of polyether polyol / bisphenol epoxy resin at a first insulation temperature T1 for standby use;
[0020] Step b, preparing a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture: the number of parts Y of the aliphatic polyamine used is calculated from the number of parts X of the bisphenol epoxy resin in step a according to the formula Y=W*0.01*X, W=EM / n·a, wherein W is the weight of amine for 100 parts of the epoxy resin, E is the epoxy value of the epoxy resin, M is the molecular weight of the aliphatic polyamine, n is the number of active hydrogen atoms of the aliphatic polyamine, and a is the purity of the aliphatic polyamine;
[0021] The stirring rate of the mixing kettle is set to the second stirring rate, and Y parts of the aliphatic polyamine are sequentially added into the polyether polyol / bisphenol epoxy resin liquid mixture prepared in step a according to preset batches, and stirred for 5 to 10 minutes to obtain a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture, and the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture is kept warm at the second insulation temperature T2 for standby use;
[0022] Step c, preparing a solid-liquid phase change composite material: putting the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture prepared in step b into a target container, and keeping it warm at a third insulation temperature T3 for more than 30 minutes, and then cooling it to room temperature to obtain a solid-liquid phase change composite material.
[0023] Further, the melting point temperature of the polyether polyol is T;
[0024] In step a, the preset temperature T0, T+5°C≤T0≤T+10°C;
[0025] And / or, in step a, the first insulation temperature T1, T+5°C≤T1≤T+15°C;
[0026] And / or, in step b, the second insulation temperature T2, T+5°C≤T2≤T+15°C;
[0027] And / or, in step c, the second insulation temperature T3, T+5°C≤T3≤T+15°C.
[0028] Furthermore, in step a, the first stirring rate of the mixing kettle is set to 30 to 50 rpm;
[0029] And / or, in step c, the second stirring rate of the mixing kettle is set to be greater than or equal to 300 rpm.
[0030] Furthermore, in step b, the preset batch is at least twice.
[0031] The technical solution provided by the embodiment of the present invention has the following beneficial effects:
[0032] (1) The solid-liquid phase change composite material provided in the embodiments of the present invention has basically no liquid leakage when the solid-liquid phase change occurs, and will not melt after heating. The loading efficiency of the solid-liquid phase change material can reach more than 94.5%, which is much higher than the 70% loading limit of the existing solid-liquid phase change material research and practical application. The latent heat of phase change is large, and it still has phase change characteristics after undergoing 1000 heating / cooling cycles.
[0033] (2) The preparation method of the solid-liquid phase change composite material provided in the embodiment of this aspect can prepare a phase change composite material with stable morphology and no leakage during solid-liquid phase change. The preparation process only involves heating and dispersion, the process is simple and efficient, and the preparation facility requirements are low. It does not require the use of solvents and other chemicals, and is economical and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a scanning electron microscope (SEM) image of the solid-liquid phase change composite material prepared in Example 1 of the present invention.
[0035] Figure 2 This is a SEM image of the solid-liquid phase change composite material prepared in Example 5 of the present invention.
[0036] Figure 3 This is a schematic diagram of the differential scanning calorimetry (DSC) scanning results of the solid-liquid composite variable material prepared in Examples 1-5 of the present invention.
[0037] Figure 4 Schematic diagram of DSC scanning results of the solid-liquid phase change composite material prepared in Example 1 of the present invention before and after undergoing 1000 heating / cooling cycles.
[0038] Figure 5 Schematic diagram of DSC scanning results of the solid-liquid phase change composite material prepared in Example 3 of the present invention before and after undergoing 1000 heating / cooling cycles. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] In addition, it should be understood that after reading the contents disclosed in the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the protection scope defined by the present invention.
[0041] In a first aspect, an embodiment of the present invention provides a solid-liquid phase change composite material, wherein the solid-liquid phase change composite material is prepared by inducing phase separation through reaction of a thermosetting resin and a polyamine in a polyol.
[0042] It should be noted that the polyol described in the present application has phase change characteristics and is the main material, which plays the functions of absorbing, storing and releasing heat. The thermosetting resin and the polyamine can react with each other and play a supporting and molding stabilizing role. The polyol can be evenly dispersed in the resin matrix after the thermosetting resin and the polyamine are synthesized.
[0043] Further, the polyol includes a polyether polyol;
[0044] The general formula of the polyether polyol is H-(OC4H8)n-OH, where n≥3, and n is an integer, for example, n can be 3, 8, 13, 27, 41, 55, etc.
[0045] Further, the thermosetting resin includes epoxy resin;
[0046] The epoxy resin includes bisphenol epoxy resin;
[0047] The bisphenol epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AD epoxy resin, bisphenol S epoxy resin, hydroxymethyl bisphenol A epoxy resin, and resorcinol epoxy resin;
[0048] Further, the polyamine includes aliphatic polyamine;
[0049] The general formula of the aliphatic polyamine is H2N(-C n H 2n )x-(NH)y-NH2,n≥2,x≥1,y≥0,
[0050] The aliphatic polyamine includes at least one of diethylenetriamine (H2N-C2H4-NH-C2H4-NH2, DETA), triethylenetetramine (H2N-C2H4-NH-C2H4-NH-C2H4-NH2, TETA), tetraethylenepentamine (H2N-C2H4-(NH-C2H4)3-NH2, TEPA), ethylenediamine (H2N-C2H4-NH2, EDA), and 1,6-hexanediamine (NH2-(C2H4)3-NH2, HMD);
[0051] Furthermore, calculated by weight, the solid-liquid phase change composite material comprises:
[0052] 100 parts of polyether polyol;
[0053] X parts of bisphenol epoxy resin, 5≤X≤20; for example, it can be 5 parts, 10 parts, 15 parts, 20 parts, etc., Y parts of aliphatic polyamine, Y=W*0.01*X,
[0054] Wherein, W=EM / n·a, W is the weight percentage of the aliphatic polyamine used in 100 parts of the bisphenol-type epoxy resin, E is the epoxy value of the bisphenol-type epoxy resin, M is the molecular weight of the aliphatic polyamine, n is the number of active hydrogen atoms of the aliphatic polyamine, and a is the purity (%) of the aliphatic polyamine.
[0055] In a specific embodiment, the solid-liquid phase change composite material uses 5 parts (i.e., X=5) of bisphenol A epoxy resin, calculated by weight, then E=0.53, M=103, n=5, a=98%, W=EM / n·a=0.53*103 / 5*0.98=10.7, Y=W*0.01*X=10.7*0.05=0.53, and it is calculated that 0.53 parts of DETA need to be added;
[0056] In another specific embodiment, the solid-liquid phase change composite material uses 10 parts (i.e., X=10) of bisphenol A epoxy resin, calculated by weight, then E=0.53, M=103, n=5, a=98%, W=EM / n·a=0.53*103 / 5*0.98=10.7, Y=W*0.01*X=10.7*0.10=1.07, and it is calculated that 1.07 parts of DETA need to be added;
[0057] In another specific embodiment, the solid-liquid phase change composite material uses 15 parts (i.e., X=15) of bisphenol A epoxy resin, calculated by weight, then E=0.53, M=103, n=5, a=98%, W=EM / n·a=0.53*103 / 5*0.98=10.7, Y=W*0.01*X=10.7*0.15=1.60, and it is calculated that 1.60 parts of DETA need to be added;
[0058] In another specific embodiment, the solid-liquid phase change composite material uses 20 parts (i.e., X=20) of bisphenol A epoxy resin, calculated by weight, then E=0.53, M=103, n=5, a=98%, W=EM / n·a=0.53*103 / 5*0.98=10.7, Y=W*0.01*X=10.7*0.20=2.14, and it is calculated that 2.14 parts of DETA need to be added.
[0059] In a second aspect, an embodiment of the present invention provides a method for preparing a solid-liquid phase change composite material, comprising the following steps:
[0060] Step a, preparing a liquid mixture of polyether polyol / bisphenol epoxy resin: by weight, putting 100 parts of solid polyether polyol and X parts (5≤X≤20) of bisphenol epoxy resin into a mixing kettle, setting the stirring rate of the mixing kettle to a first stirring rate, and heating the mixture to a preset temperature T0 so that the mixture is a transparent and uniform liquid, to obtain a liquid mixture of polyether polyol / bisphenol epoxy resin, and keeping the liquid mixture of polyether polyol / bisphenol epoxy resin at a first insulation temperature T1 for standby use;
[0061] It should be noted that the solid polyether polyol and the bisphenol epoxy resin are first heated and mixed into a transparent and uniform liquid in order to improve the uniform dispersion of the bisphenol epoxy resin in the polyether polyol, which is beneficial for the aliphatic polyamine and the epoxy resin to achieve molecular-level mixed contact in the subsequent steps, thereby causing a uniform curing reaction.
[0062] Step b, preparing a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture: the number of parts Y of the aliphatic polyamine used is calculated from the number of parts X of the bisphenol epoxy resin in step a according to the formula Y=W*0.01*X, W=EM / n·a, wherein W is the weight of amine for 100 parts of the epoxy resin, E is the epoxy value of the epoxy resin, M is the molecular weight of the aliphatic polyamine, n is the number of active hydrogen atoms of the aliphatic polyamine, and a is the purity of the aliphatic polyamine;
[0063] The stirring rate of the mixing kettle is set to the second stirring rate, and Y parts of the aliphatic polyamine are sequentially added into the polyether polyol / bisphenol epoxy resin liquid mixture prepared in step a according to preset batches, and stirred for 5 to 10 minutes, for example, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, etc., to obtain a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture, and the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture is kept warm at the second insulation temperature T2 for standby use;
[0064] First, the polyether polyol and the bisphenol epoxy resin are mixed evenly, and then the aliphatic polyamine is added in batches under high-speed dispersion conditions. On the one hand, because the reaction speed of the bisphenol epoxy resin and the aliphatic polyamine is very fast, especially the reaction rate is faster under heating conditions, adding the aliphatic polyamine in batches under high-speed dispersion can extend the operation time and reduce the occurrence of local reactions; on the other hand, adding the aliphatic polyamine in batches can increase the dispersion of the aliphatic polyamine in the polyether polyol / bisphenol epoxy resin liquid mixture, which is beneficial to reduce the particle size of the phase generated by the reaction-induced phase separation and improve the morphological stability of the final polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture. The reaction of the bisphenol epoxy resin and the aliphatic polyamine is as follows:
[0065]
[0066] Step c, preparing a solid-liquid phase change composite material: putting the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture prepared in step b into a target container, and keeping it warm at a third insulation temperature T3 for more than 30 minutes, for example, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 120 minutes, etc., and then cooling it to room temperature to obtain a solid-liquid phase change composite material.
[0067] In the present application, the type of the target container is not limited, such as molds, mechanical structures, equipment, etc. with complex internal structures. Since the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture in step b is a liquid with low viscosity and good fluidity, after it is flowed into the target container, it is kept warm and cooled to form, and the solid-liquid phase change composite material of any structure can be obtained. The preparation process is not limited by the shape of the actual application mold, equipment, place, etc., and can be formed in any structure, with strong adaptability and a wide range of applications.
[0068] Further, the melting point temperature of the polyether polyol is T;
[0069] In step a, the preset temperature T0, T+5°C≤T0≤T+10°C;
[0070] And / or, in step a, the first insulation temperature T1, T+5°C≤T1≤T+15°C;
[0071] And / or, in step b, the second insulation temperature T2, T+5°C≤T2≤T+15°C;
[0072] And / or, in step c, the second insulation temperature T3, T+5°C≤T3≤T+15°C.
[0073] In step a to step c, T1, T2, and T3 are set to be 5 to 15° C. higher than the melting point of the polyether polyol used, for example, 5° C., 7° C., 9° C., 11° C., 13° C., 15° C., etc. On the one hand, this is to maintain the liquid state of the entire mixture, give it good fluidity and wettability, and facilitate different practical application scenarios, such as filling and molding of complex structures and substrates containing grooves, deep grooves, gaps, etc.; on the other hand, this is to reduce the solubility of the reaction product of the polyether polyol and the bisphenol epoxy resin / aliphatic polyamine, so as to facilitate the occurrence of reaction-induced phase separation.
[0074] Furthermore, in step a, the first stirring rate of the mixing kettle is set to 30-50 rpm, for example, 30 rpm, 35 rpm, 40 rpm, 45 rpm, 50 rpm, etc.;
[0075] And / or, in step c, the second stirring rate of the mixing kettle is set to be greater than or equal to 300 rpm, for example, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, etc.
[0076] Furthermore, in step b, the preset batch is at least twice, for example, 3 times, 4 times, 5 times, 6 times, 7 times, etc.
[0077] In the following specific examples, the operations involved, if the conditions are not specified, are all carried out under conventional conditions or the conditions recommended by the manufacturer. All raw materials, if the manufacturers and specifications are not specified, are conventional products that can be obtained through commercial purchase.
[0078] The tetrahydrofuran homopolyethers (PTMG650, PTMG1000, PTMG2000) in Examples 1-5 were all purchased from Mitsubishi Chemical Corporation, and the polytetrahydrofuran (PTMEG1000) in the comparative example was purchased from BASF PolyTHF1000.
[0079] Example 1
[0080] A method for preparing a solid-liquid phase change composite material comprises the following steps:
[0081] Step a, preparing a polyether polyol / bisphenol epoxy resin liquid mixture: by weight, putting 100 parts of tetrahydrofuran homopolyether PTMG650 (H-(OC4H8)n-OH, n=8, MW=650, MP=19°C) and 5 parts of bisphenol A epoxy resin (E=0.53) into a mixing kettle, setting a first stirring rate of 30 rpm, and heating to 29°C at the same time so that the mixture is a transparent liquid to obtain a polyether polyol / bisphenol epoxy resin liquid mixture, and keeping the polyether polyol / bisphenol epoxy resin liquid mixture at 24°C for standby use;
[0082] Step b, preparing a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture: setting the second stirring rate to 300 rpm, and adding 0.53 parts of DETA by weight into the polyether polyol / bisphenol epoxy resin liquid mixture prepared in step a (X=5, M=103, n=5, a=98%, W=EM / n·a=0.53*103 / 5*0.98=10.7, Y=W*0.01*X=10.7*0.05=0.53) in three portions, stirring for 5 minutes to obtain a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture, and keeping the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture warm at 24° C. for standby use;
[0083] Step c, preparing a solid-liquid phase change composite material: putting the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture prepared in step b into a target container, keeping it warm at 24° C. for 30 minutes, and then cooling it to room temperature to obtain a solid-liquid phase change composite material.
[0084] Example 2
[0085] A method for preparing a solid-liquid phase change composite material comprises the following steps:
[0086] Step a, preparing a liquid polyether polyol / bisphenol epoxy resin mixture: by weight, putting 100 parts of PTMG1000 (H-(OC4H8)n-OH, wherein n=13, MW=1000, MP=24°C) and 5 parts of bisphenol A epoxy resin (E=0.53) into a mixing kettle, setting a first stirring rate of 30 rpm, and heating to 29°C so that the mixture is a transparent liquid to obtain a polyether polyol / bisphenol epoxy resin liquid mixture, and keeping the polyether polyol / bisphenol epoxy resin liquid mixture at 30°C for standby use;
[0087] Step b, preparing a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture: setting the second stirring rate to 300 rpm, and adding 0.53 parts of DETA by weight into the polyether polyol / bisphenol epoxy resin liquid mixture prepared in step a (X=5, M=103, n=5, a=98%, W=EM / n·a=0.53*103 / 5*0.98=10.7, Y=W*0.01*X=10.7*0.05=0.53) in three portions, stirring for 5 minutes to obtain a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture, and keeping the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture warm at 30° C. for standby use;
[0088] Step c, preparing a solid-liquid phase change composite material: putting the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture prepared in step b into a target container, keeping it at 30° C. for 30 minutes, and then cooling it to room temperature to obtain a solid-liquid phase change composite material.
[0089] Example 3
[0090] A method for preparing a solid-liquid phase change composite material comprises the following steps:
[0091] Step a, preparing a liquid polyether polyol / bisphenol epoxy resin mixture: by weight, putting 100 parts of PTMG2000 (H-(OC4H8)n-OH, n=27, MW=2000, MP=32°C) and 5 parts of bisphenol A epoxy resin (E=0.53) into a mixing kettle, setting a first stirring rate of 40 rpm, and heating to 42°C at the same time, so that the mixture is a transparent liquid, to obtain a polyether polyol / bisphenol epoxy resin liquid mixture, and keeping the polyether polyol / bisphenol epoxy resin liquid mixture at 40°C for standby use;
[0092] Step b, preparing a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture: setting the second stirring rate to 300 rpm, and adding 0.53 parts of DETA by weight into the polyether polyol / bisphenol epoxy resin liquid mixture prepared in step a (X=5, M=103, n=5, a=98%, W=EM / n·a=0.53*103 / 5*0.98=10.7, Y=W*0.01*X=10.7*0.05=0.53) in three portions, stirring for 10 minutes to obtain a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture, and keeping the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture at 40° C. for standby use;
[0093] Step c, preparing a solid-liquid phase change composite material: putting the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture prepared in step b into a target container, keeping it at 40° C. for 30 minutes, and then cooling it to room temperature to obtain a solid-liquid phase change composite material.
[0094] Example 4
[0095] A method for preparing a solid-liquid phase change composite material comprises the following steps:
[0096] Step a, preparing a liquid polyether polyol / bisphenol epoxy resin mixture: by weight, putting 100 parts of PTMG1000 (H-(OC4H8)n-OH, n=13, MW=1000, MP=24°C) and 5 parts of bisphenol F epoxy resin (E=0.54) into a mixing kettle, setting a first stirring rate of 30 rpm, and heating to 30°C at the same time so that the mixture is a transparent liquid to obtain a polyether polyol / bisphenol epoxy resin liquid mixture, and keeping the polyether polyol / bisphenol epoxy resin liquid mixture at 30°C for standby use;
[0097] Step b, preparing a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture: setting the second stirring rate to 300 rpm, and adding 0.57 parts of DETA by weight into the polyether polyol / bisphenol epoxy resin liquid mixture prepared in step a (X=5, M=103, n=5, a=98%, W=EM / n·a=0.54*103 / 5*0.98=11.4, Y=W*0.01*X=11.4*0.05=0.57) in three portions, stirring for 5 minutes to obtain a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture, and keeping the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture warm at 30° C. for standby use;
[0098] Step c, preparing a solid-liquid phase change composite material: putting the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture prepared in step b into a target container, keeping it at 30° C. for 30 minutes, and then cooling it to room temperature to obtain a solid-liquid phase change composite material.
[0099] Example 5
[0100] A method for preparing a solid-liquid phase change composite material comprises the following steps:
[0101] Step a, preparing a liquid polyether polyol / bisphenol epoxy resin mixture: by weight, putting 100 parts of PTMG2000 (H-(OC4H8)n-OH, n=27, MW=2000, MP=32°C) and 20 parts of bisphenol F epoxy resin (E=0.54) into a mixing kettle, setting a first stirring rate of 50 rpm, and heating to 42°C at the same time so that the mixture is a transparent liquid to obtain a polyether polyol / bisphenol epoxy resin liquid mixture, and keeping the polyether polyol / bisphenol epoxy resin liquid mixture at 35°C for standby use;
[0102] Step b, preparing a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture: setting the second stirring rate to 400 rpm, and adding 2.68 parts of TETA by weight into the polyether polyol / bisphenol epoxy resin liquid mixture prepared in step a (X=20, M=146, n=6, a=98%, W=EM / n·a=0.54*146 / 6*0.98=13.4, Y=W*0.01*X=13.4*0.2=2.68) in 4 portions, stirring for 5 minutes to obtain a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture, and keeping the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture at 30° C. for standby use;
[0103] Step c, preparing a solid-liquid phase change composite material: putting the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture prepared in step b into a target container, keeping it at 30° C. for 30 minutes, and then cooling it to room temperature to obtain a solid-liquid phase change composite material.
[0104] Comparative Example
[0105] Commercially available polytetrahydrofuran (PTMEG1000) was selected.
[0106] Application Examples
[0107] This application example tests the heating morphology, phase change temperature, phase change enthalpy and solid-liquid phase change weight change of the solid-liquid phase change composite material prepared in Example 2 and Example 4 and the PTMEG1000 provided in the comparative example. The specific phase change test parameters of the solid-liquid phase change composite material prepared in Example 2 and Example 4 and the comparative example PTMEG1000 are shown in Table 1 below.
[0108] Table 1 Test results of Example 2, Example 4 and Comparative Example PTMEG1000
[0109]
[0110] It can be seen from Table 1 that the weight change of the solid-liquid phase change composite materials prepared in Examples 2 and 4 of the present invention when the solid-liquid phase change occurs is very small, with only a decrease of 0.1%, which means that there is basically no liquid leakage when the solid-liquid phase change occurs. At the same time, the loading efficiency of the solid-liquid phase change material can reach more than 94.5%, which is much greater than the 70% loading upper limit of the existing solid-liquid phase change material research and practical application, which also leads to a larger phase change enthalpy.
[0111] Depend on Figure 1 and Figure 2 It can be seen that the solid-liquid phase change composite materials prepared in Example 1 and Example 5 of the present invention have microscopic particles with relatively uniform sizes.
[0112] Depend on Figure 3 It can be seen that the solid-liquid phase change composite materials prepared in Examples 1-5 of the present invention and the PTMEG1000 provided in the comparative example both exhibit obvious phase change characteristics, namely, endothermic behavior when heated and exothermic behavior when cooled.
[0113] Depend on Figure 4 and Figure 5 It can be seen that the solid-liquid phase change composite materials prepared in Example 1 and Example 3 still have phase change characteristics after being subjected to 1000 heating / cooling cycles, and the absorption peaks of the phase change before and after do not change much.
[0114] In addition, the solid-liquid phase change composite materials prepared in Example 1, Example 2 and Example 5 and the comparative example were heated to 60°C. The PTMEG1000 provided in the comparative example gradually melted into a transparent liquid after heating, while the composite materials prepared in Example 1, Example 2 and Example 5 maintained their morphology unchanged after heating.
[0115] The above can prove that the preparation method of the solid-liquid phase change composite material provided in the embodiment of the present invention can prepare a phase change composite material with stable morphology and no leakage during solid-liquid phase change, and the preparation facility requirements are low, the process is simple and efficient, and no solvents or other chemicals are required, which is economical and environmentally friendly.
[0116] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A solid-liquid phase change composite material, characterized in that: The solid-liquid phase change composite material is prepared by inducing phase separation through reaction between thermosetting resin and polyamine in polyol.
2. The solid-liquid phase change composite material according to claim 1, characterized in that: The polyol comprises a polyether polyol; The general formula of the polyether polyol is H-(OC4H8)n-OH, where n≥3.
3. The solid-liquid phase change composite material according to claim 1, characterized in that: The thermosetting resin includes epoxy resin; The epoxy resin includes bisphenol epoxy resin; The bisphenol epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AD epoxy resin, bisphenol S epoxy resin, hydroxymethyl bisphenol A epoxy resin, and resorcinol epoxy resin.
4. The solid-liquid phase change composite material according to claim 1, characterized in that: The polyamine includes aliphatic polyamine; The general formula of the aliphatic polyamine is H2N(-C n H 2n )x-(NH)y-NH2,n≥2,x≥1,y≥0, The aliphatic polyamine includes at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine, ethylenediamine, and 1,6-hexanediamine.
5. The solid-liquid phase change composite material according to claim 1, characterized in that: Calculated by weight, the solid-liquid phase change composite material comprises: 100 parts of polyether polyol; X parts of bisphenol epoxy resin, 5≤X≤20; Y parts of aliphatic polyamine, Y=W*0.01*X, Wherein, W=EM / n·a, W is the weight percentage of the aliphatic polyamine used for 100 parts of the bisphenol epoxy resin, E is the epoxy value of the bisphenol epoxy resin, M is the molecular weight of the aliphatic polyamine, n is the number of active hydrogen atoms of the aliphatic polyamine, and a is the purity (%) of the aliphatic polyamine.
6. A method for preparing a solid-liquid phase change composite material, characterized in that: The method for preparing the solid-liquid phase change composite material according to any one of claims 1 to 5 comprises the following steps: Step a, preparing a liquid mixture of polyether polyol / bisphenol epoxy resin: by weight, putting 100 parts of solid polyether polyol and X parts (5≤X≤20) of bisphenol epoxy resin into a mixing kettle, setting the stirring rate of the mixing kettle to a first stirring rate, and heating the mixture to a preset temperature T0 so that the mixture is a transparent and uniform liquid, to obtain a liquid mixture of polyether polyol / bisphenol epoxy resin, and keeping the liquid mixture of polyether polyol / bisphenol epoxy resin at a first insulation temperature T1 for standby use; Step b, preparing a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture: the number of parts Y of the aliphatic polyamine used is calculated from the number of parts X of the bisphenol epoxy resin in step a according to the formula Y=W*0.01*X, W=EM / n·a, wherein W is the weight of amine for 100 parts of the epoxy resin, E is the epoxy value of the epoxy resin, M is the molecular weight of the aliphatic polyamine, n is the number of active hydrogen atoms of the aliphatic polyamine, and a is the purity of the aliphatic polyamine; The stirring rate of the mixing kettle is set to the second stirring rate, and Y parts of the aliphatic polyamine are sequentially added into the polyether polyol / bisphenol epoxy resin liquid mixture prepared in step a according to preset batches, and stirred for 5 to 10 minutes to obtain a polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture, and the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture is kept warm at the second insulation temperature T2 for standby use; Step c, preparing a solid-liquid phase change composite material: putting the polyether polyol / bisphenol epoxy resin / aliphatic polyamine mixture prepared in step b into a target container, and keeping it warm at a third insulation temperature T3 for more than 30 minutes, and then cooling it to room temperature to obtain a solid-liquid phase change composite material.
7. The solid-liquid phase change composite material according to claim 6, characterized in that: The melting point temperature of the polyether polyol is T; In step a, the preset temperature T0, T+5°C≤T0≤T+10°C; And / or, in step a, the first insulation temperature T1, T+5°C≤T1≤T+15°C; And / or, in step b, the second insulation temperature T2, T+5°C≤T2≤T+15°C; And / or, in step c, the second insulation temperature T3, T+5°C≤T3≤T+15°C.
8. The solid-liquid phase change composite material according to claim 6, characterized in that: In step a, the first stirring rate of the mixing kettle is set to 30-50 rpm; And / or, in step c, the second stirring rate of the mixing kettle is set to be greater than or equal to 300 rpm.
9. The solid-liquid phase change composite material according to claim 6, characterized in that: In step b, the preset batch is at least twice.