Sheath material for cable of maglev train as well as manufacturing method and application of sheath material
By combining thermoplastic polyurethane elastomer and new phosphorus-nitrogen flame retardant and using step-by-step blending technology, the high flame retardant, high mechanical properties and mildew resistance of magnetic levitation train cables in complex environments is achieved, and excellent Comprehensive performance to meet the needs of high-speed trains.
Patent Information
- Application Number
- CN202411115741.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
Smart Images

Figure BDA0004993567980000021 
Figure BDA0004993567980000051 
Figure BDA0004993567980000052
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials and engineering technology, and in particular to a cable sheath material with high flame retardancy, high mechanical properties and high mildew resistance for maglev train cables, and a manufacturing method and application thereof. Background Art
[0002] The cables used in 620 km / h maglev trains are in a complex and harsh environment for a long time, and there is a certain degree of wear during operation. In order to reduce wear and increase the service life of the cables, it is of great significance to develop a sheath material with high flame retardancy, high mechanical properties, and high mildew resistance.
[0003] Patent CN201810825287.X uses melamine and 2,3-epoxypropyltrimethylammonium chloride as raw materials to prepare hydroxypropyltrimethylammonium chloride melamine flame retardant to enhance the flame retardant properties of the material. Patent CN 201910957451.7 uses cyanuric chloride and p-hydroxybenzaldehyde to synthesize 2,4,6-tris(4-formylphenoxy)-1,3,5-triazine, and then 2,4,6-tris(4-formylphenoxy)-1,3,5-triazine, p-aminophenol and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to synthesize tris-[4-(p-hydroxyaniline-phosphaphenanthrene)methylene-phenoxy]-1,3,5-triazine flame retardant, triazine six-membered heterocyclic ring (N source) as the core, DOPO group as the P source, to improve the flame retardant properties of the material. However, the main purpose of the above technologies is to improve flame retardancy, which has caused a certain degree of decline in the mechanical properties of the materials. The improvement of material performance is relatively simple and it is difficult to meet the application requirements in complex and harsh environments.
[0004] At present, most of the technologies related to cable products used in domestic maglev trains are mastered by foreign countries. It is of great significance to develop cable sheath materials with high flame retardancy, high mechanical properties and high mildew resistance for maglev train cables with independent intellectual property rights. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a cable sheath material with high flame retardancy, high mechanical properties and high mildew resistance for maglev train cables, and a manufacturing method and application thereof.
[0006] The present invention adopts the following technical solutions to solve the above technical problems:
[0007] A sheath material for a maglev train cable comprises the following raw materials in parts by weight: 100-150 parts of thermoplastic polyurethane elastomer (TPU), 30-50 parts of a novel phosphorus-nitrogen flame retardant, 40-60 parts of a reinforcing filler, 1.5-2.5 parts of a stabilizer, 10-20 parts of a carbonizing agent, 10-15 parts of a smoke suppressant, 5-10 parts of a mildew preventer, 1.5-3 parts of an antioxidant, 1-1.5 parts of an anti-aging agent, and 1-5 parts of a masterbatch;
[0008] The novel phosphorus-nitrogen flame retardant is a phenanthrene cyclotriazine cyanide DMMDI containing a 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide unit and a triazine structure, and the structural formula is shown in the following formula I:
[0009]
[0010] In Formula I, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms.
[0011] As one of the preferred embodiments of the present invention, the density of the thermoplastic polyurethane elastomer (TPU) is 1.10 to 1.14 g / cm 3 , melting point 140 ~ 150 ℃, Shore hardness (A) 84 ~ 90, the hard segment contains a benzene ring structure, and the soft segment contains an ether bond structure.
[0012] As one of the preferred embodiments of the present invention, the reinforcing filler is one or more of calcium carbonate, talc, and kaolinite, and more preferably a mixture of calcium carbonate and kaolinite.
[0013] As one of the preferred embodiments of the present invention, the stabilizer is one or more of calcium stearate, barium stearate, and zinc stearate, and more preferably a mixture of barium stearate and calcium stearate.
[0014] As one of the preferred embodiments of the present invention, the carbon-forming agent is one or more of piperazine pyrophosphate, trimethylolethane, and pentaerythritol, and more preferably a mixture of pentaerythritol and trimethylolethane.
[0015] As one of the preferred embodiments of the present invention, the smoke suppressant is one or more of ammonium dimolybdate, calcium phosphomolybdate, hydroxide, and ammonium octamolybdate, and more preferably a mixture of ammonium dimolybdate and ammonium octamolybdate.
[0016] As one of the preferred embodiments of the present invention, the antifungal agent is one or more of zinc ions, silver ions, copper ion compounds, and calcium phosphate, and more preferably a mixture of cuprous oxide and calcium phosphate.
[0017] As one of the preferred embodiments of the present invention, the antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol, 2,2′-thiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N′-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, and tris[2,4-di-tert-butylphenyl]phosphite. More preferably, it is a mixture of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol and N,N′-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine.
[0018] As one of the preferred embodiments of the present invention, the antioxidant is one or more of 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, N,N′-di(β-naphthyl)-p-phenylenediamine, N,N′-diphenyl-p-phenylenediamine, and N-phenyl-β-naphthylamine. More preferably, it is a mixture of 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and N,N′-di(β-naphthyl)-p-phenylenediamine.
[0019] A method for manufacturing the sheath material for the above-mentioned maglev train cable: adding thermoplastic polyurethane elastomer, novel phosphorus-nitrogen flame retardant, carbonizing agent, smoke suppressant, antioxidant, stabilizer and reinforcing filler into an internal mixer for melt blending; after cooling and drying, placing the above-mentioned mixture into a twin-screw extruder for melt blending and extrusion; after cooling and drying, obtaining a blended masterbatch; adding the above-mentioned blended masterbatch, color masterbatch, antioxidant and mildewproof agent into a high-speed mixer for mixing; then placing it into a twin-screw extruder for melt blending and extrusion; after cooling and drying, obtaining a cross-linked masterbatch; placing the above-mentioned cross-linked masterbatch into a wire and cable extruder for melt extrusion to obtain a cross-linked cable; irradiating the cross-linked cable to obtain a finished cable.
[0020] As one of the preferred embodiments of the present invention, first, a thermoplastic polyurethane elastomer, a novel phosphorus-nitrogen flame retardant, a carbonizing agent, a smoke suppressant, an antioxidant, a stabilizer, and a reinforcing filler are added to an internal mixer, and melt-blended for 10 minutes at 185° C. and 50 rpm; after cooling and drying, the mixture is placed in a twin-screw extruder at a temperature of 140 to 185° C. for melt-blending and extrusion, preferably 175 to 185° C.; after cooling and drying, a blended masterbatch is obtained;
[0021] The above blended masterbatch, color masterbatch, antioxidant and mildewproof agent are added into a high-speed mixer and mixed for 15 minutes at 2500-4000 r / min; the mixture is placed in a twin-screw extruder at a temperature of 140-185°C for melt blending and extrusion, preferably 175-185°C; after cooling and drying, a cross-linked masterbatch is obtained;
[0022] The cross-linked masterbatch is placed in a wire and cable extruder at a temperature of 140 to 190° C. for melt extrusion, preferably 140 to 185° C., to obtain a cross-linked cable; the cross-linked cable is irradiated for 10 minutes under the conditions of a beam pressure of 1.5 to 2 MeV, a beam current of 40 mA, and an irradiation dose of 300 kGy to obtain a finished cable.
[0023] As one of the preferred embodiments of the present invention, the step of preparing the novel phosphorus-nitrogen flame retardant is also included:
[0024] Melamine, N,N-dimethylformamide and 4-dimethylaminopyridine catalyst are added to a three-necked flask, and heated and stirred under a nitrogen atmosphere to completely dissolve them; p-olefin benzene carboxylic acid is then dissolved in N,N-dimethylformamide, added dropwise to the three-necked flask, and heated and stirred until the reaction is completed; after the reaction is completed, the reaction mixture is poured into excess deionized water to precipitate to obtain an intermediate product, which is then washed, rotary evaporated, and dried to obtain a triazine structure compound MCO represented by formula II:
[0025]
[0026] In formula II, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms;
[0027] DOPO, 4,4′-methylenebis(phenyl isocyanate) and toluene are added to a three-necked flask and heated and stirred to completely dissolve, and then the triazine structure compound MCO is added, and heated and stirred until the reaction is completed; after the reaction is completed, the mixture is cooled to room temperature, filtered, washed and dried to obtain a novel phosphorus-nitrogen flame retardant DMMDI shown in Formula I:
[0028]
[0029] In Formula I, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms.
[0030] As one of the preferred methods of the present invention, melamine, N,N-dimethylformamide and 4-dimethylaminopyridine catalyst are added to a three-necked flask, stirred and heated to 85°C under a nitrogen atmosphere to completely dissolve them; then, p-olefin benzene carboxylic acid is dissolved in N,N-dimethylformamide, added dropwise to the three-necked flask, heated to maintain 85°C, and the stirring rate is controlled to be 300r / min, and the reaction is kept warm for 15 hours; after the reaction is completed, the reaction mixture is poured into an excess of deionized water to precipitate to obtain an intermediate product, and then washed, rotary evaporated, and dried to obtain a triazine structure compound MCO represented by formula II:
[0031]
[0032] In formula II, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms;
[0033] DOPO, 4,4′-methylenebis(phenyl isocyanate) and toluene were added to a three-necked flask, the system was heated to 85°C, and the stirring rate was controlled to be 300r / min; after the system was completely dissolved, the above-mentioned triazine structure compound MCO was added, and the temperature was continued to be raised to 110°C, and the reaction was kept warm for 7h; after the reaction was completed, it was cooled to room temperature, filtered, washed and dried to obtain a novel phosphorus nitrogen flame retardant DMMDI shown in formula I:
[0034]
[0035] In Formula I, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms.
[0036] An application of the above-mentioned sheath material for maglev train cables, wherein the material is applied to cables for maglev trains with a speed of 620 kilometers per hour or above and cables for intelligent equipment serving in complex environments.
[0037] The advantages of the present invention compared to the prior art are:
[0038] (1) The novel phosphorus-nitrogen flame retardant of the present invention contains DOPO flame retardant unit, triazine structure and a large number of benzene rings, is easy to form carbon, has excellent thermal stability, high flame retardant efficiency, contains MDI structure so that it has good compatibility with the matrix, has a small addition content and does not precipitate, and can improve the comprehensive performance of the material;
[0039] (2) The carbonizing agent of the present invention is a substance rich in oxygen such as trimethylolethane and pentaerythritol, which not only promotes carbonization, but also combines with the isocyanate group in the novel phosphorus-nitrogen flame retardant and plays a role in regulating the interface compatibility, thereby improving the mechanical properties of the cable sheath material;
[0040] (3) The present invention introduces inorganic mildew inhibitors such as zinc ions, silver ions, and copper ion compounds, which can effectively prevent mildew, thereby achieving an excellent long-term stable mildew-proof effect, and broadening the application field of the cable sheath material in harsh and complex environments;
[0041] (4) The material of the present invention is prepared by step-by-step blending, and the shearing action between different melt strength gradients leads to uniform dispersion of the filler, thereby finally obtaining a cable sheath material with excellent comprehensive performance. DETAILED DESCRIPTION
[0042] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.
[0043] About the raw materials used in the following examples:
[0044] Thermoplastic polyurethane elastomer (TPU): density 1.12g / cm 3 , melting point is 140~150℃, Shore hardness (A) is 87, hard segment contains benzene ring structure, soft segment contains ether bond structure, tensile strength is 51MPa, elongation at break is 500~700MPa, selected from Lubrizol of the United States
[0045] A novel phosphorus-nitrogen flame retardant: a phenanthrene cyclotriazine cyanide (DMMDI) containing 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide motif in a triazine structure, the preparation of which includes the following steps:
[0046] 0.05 mol of melamine, 50 mL of N,N-dimethylformamide and 5 g of 4-dimethylaminopyridine catalyst were added to a three-necked flask, stirred and heated to 85°C under a nitrogen atmosphere to completely dissolve them; 0.151 mol of p-olefin benzene carboxylic acid was dissolved in 200 mL of N,N-dimethylformamide, added dropwise to the three-necked flask, heated to maintain 85°C, and the stirring rate was controlled to be 300 r / min, and the reaction was kept warm for 15 hours; after the reaction was completed, the reaction mixture was poured into an excess of deionized water to precipitate to obtain an intermediate product, which was then washed, rotary evaporated, and dried to obtain a triazine structure compound (MCO) represented by Formula II:
[0047]
[0048] In formula II, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms.
[0049] 0.04 mol DOPO, 0.03 mol 4,4′-methylenebis(phenyl isocyanate) and 100 mL toluene were added to a three-necked flask, the system was heated to 85°C, and the stirring rate was controlled to be 300 r / min; after the system was completely dissolved, 0.01 mol MCO of the above triazine structure compound was added, the temperature was continued to be raised to 110°C, and the reaction was kept warm for 7 hours; after the reaction was completed, the mixture was cooled to room temperature, filtered, washed and dried to obtain a novel phosphorus nitrogen flame retardant (DMMDI) shown in Formula I:
[0050]
[0051] In Formula I, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms.
[0052] Reinforcing filler: a mixture of calcium carbonate and kaolinite in a mass ratio of 2:1; calcium carbonate is selected from Shanghai Chuangsai Technology Co., Ltd., and kaolinite is selected from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0053] Stabilizer: A mixture of barium stearate and calcium stearate in a mass ratio of 1:1; the raw materials are all selected from Jinan Century Tongda Chemical Co., Ltd.
[0054] Carbon-forming agent: a mixture of pentaerythritol and trimethylolethane in a mass ratio of 1:1; the raw materials are all selected from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0055] Smoke suppressant: a mixture of ammonium dimolybdate and ammonium octamolybdate in a mass ratio of 1:1; the raw materials are all selected from Shanghai Chuangsai Technology Co., Ltd.
[0056] Antifungal agent: a mixture of cuprous oxide and calcium phosphate in a mass ratio of 1:1; the raw materials are all selected from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0057] Antioxidant: a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and N,N′-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine in a mass ratio of 1:1; wherein pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 1010 produced by American Cytec Company, and N,N′-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine is 1024 produced by Shanghai Aladdin Biochemical Technology Co., Ltd.
[0058] Antiaging agent: a mixture of 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and N,N′-di(β-naphthyl)-p-phenylenediamine in a mass ratio of 2:1; the raw materials are all selected from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0059] Masterbatch: UN6073 from Cabot Corporation of the United States is used.
[0060] Aluminum hydroxide: HT-205 produced by Jinan Taixing Fine Chemical Co., Ltd. was selected.
[0061] Magnesium hydroxide: HT-206 produced by Jinan Taixing Fine Chemical Co., Ltd. was selected.
[0062] Zinc borate: HT-207 produced by Jinan Taixing Fine Chemical Co., Ltd. was selected.
[0063] DOPO: Selected for use by Shanghai Aladdin Biochemical Technology Co., Ltd.
[0064] Melamine: Selected for use in Shanghai Aladdin Biochemical Technology Co., Ltd.
[0065] The weight proportions of the raw materials in the following examples and comparative examples are shown in Table 1.
[0066] Table 1 Raw materials and dosage of sheath materials in various embodiments and comparative examples (by weight)
[0067]
[0068]
[0069] Example 1
[0070] The sheath material for a magnetic levitation train cable of this embodiment, the raw materials and the formula are shown in Table 1.
[0071] Preparation method:
[0072] (1) A thermoplastic polyurethane elastomer, a novel phosphorus-nitrogen flame retardant, a charring agent, a smoke suppressant, an antioxidant, a stabilizer, and a reinforcing filler are added to an internal mixer, and melt-blended at 185° C. and 50 rpm for 10 min; after cooling and drying, the mixture is placed in a twin-screw extruder for melt-blending and extrusion, and the processing temperatures from the feed port to the die port are 175° C., 175° C., 180° C., 180° C., 185° C., and 185° C., respectively; after cooling and drying, a blended masterbatch is obtained.
[0073] (2) Add the above-mentioned blended masterbatch, color masterbatch, antioxidant and mildewproof agent into a high-speed mixer and mix them at 2500r / min for 15min; place them in a twin-screw extruder for melt blending and extrusion, and the processing temperatures from the feed port to the die port are 175°C, 175°C, 180°C, 180°C, 185°C and 185°C respectively; after cooling and drying, a cross-linked masterbatch is obtained.
[0074] (3) placing the cross-linked masterbatch in a wire and cable extruder for melt extrusion, with an inlet temperature of 140°C, a first section of 140-150°C, a second section of 150-160°C, a third section of 160-170°C, a fourth section of 170-175°C, a fifth section of 175-180°C, and an outlet temperature of 185°C, and coating the surface of the cable conductor core with a sheath; irradiating the coated core for 10 min under the conditions of a beam pressure of 1.5 MeV, a beam current of 40 mA, and an irradiation dose of 300 kGy to obtain a finished cable.
[0075] Example 2
[0076] The sheath material for a magnetic levitation train cable of this embodiment, the raw materials and the formula are shown in Table 1.
[0077] Preparation method:
[0078] (1) A thermoplastic polyurethane elastomer, a novel phosphorus-nitrogen flame retardant, a charring agent, a smoke suppressant, an antioxidant, a stabilizer, and a reinforcing filler are added to an internal mixer, and melt-blended at 185° C. and 50 rpm for 10 min; after cooling and drying, the mixture is placed in a twin-screw extruder for melt-blending and extrusion, and the processing temperatures from the feed port to the die port are 175° C., 175° C., 180° C., 180° C., 185° C., and 185° C., respectively; after cooling and drying, a blended masterbatch is obtained.
[0079] (2) Add the above-mentioned blended masterbatch, color masterbatch, antioxidant and mildewproof agent into a high-speed mixer and mix them at 3000 r / min for 15 min; place them in a twin-screw extruder for melt blending and extrusion, and the processing temperatures from the feed port to the die port are 175° C., 175° C., 180° C., 180° C., 185° C. and 185° C., respectively; after cooling and drying, a cross-linked masterbatch is obtained.
[0080] (3) placing the cross-linked masterbatch in a wire and cable extruder for melt extrusion, wherein the inlet temperature is 140°C, the first section is 140-150°C, the second section is 150-160°C, the third section is 160-170°C, the fourth section is 170-175°C, the fifth section is 175-180°C, and the outlet temperature is 185°C; coating the surface of the cable conductor core with a sheath; irradiating the coated core for 10 minutes under the conditions of a beam pressure of 1.8 MeV, a beam current of 40 mA, and an irradiation dose of 300 kGy to obtain a finished cable.
[0081] Example 3
[0082] The sheath material for a magnetic levitation train cable of this embodiment, the raw materials and the formula are shown in Table 1.
[0083] Preparation method:
[0084] (1) A thermoplastic polyurethane elastomer, a novel phosphorus-nitrogen flame retardant, a charring agent, a smoke suppressant, an antioxidant, a stabilizer, and a reinforcing filler are added to an internal mixer, and melt-blended at 185° C. and 50 rpm for 10 min; after cooling and drying, the mixture is placed in a twin-screw extruder for melt-blending and extrusion, and the processing temperatures from the feed port to the die port are 175° C., 175° C., 180° C., 180° C., 185° C., and 185° C., respectively; after cooling and drying, a blended masterbatch is obtained.
[0085] (2) Add the above-mentioned blended masterbatch, color masterbatch, antioxidant and mildewproof agent into a high-speed mixer and mix them at 4000 r / min for 15 min; place them in a twin-screw extruder for melt blending and extrusion, and the processing temperatures from the feed port to the die port are 175° C., 175° C., 180° C., 180° C., 185° C. and 185° C., respectively; after cooling and drying, a cross-linked masterbatch is obtained.
[0086] (3) placing the cross-linked masterbatch in a wire and cable extruder for melt extrusion, with an inlet temperature of 140°C, a first section of 140-150°C, a second section of 150-160°C, a third section of 160-170°C, a fourth section of 170-175°C, a fifth section of 175-180°C, and an outlet temperature of 185°C, and coating the surface of the cable conductor core with a sheath; irradiating the coated core for 10 min under the conditions of a beam pressure of 2 MeV, a beam current of 40 mA, and an irradiation dose of 300 kGy to obtain a finished cable.
[0087] Example 4
[0088] The sheath material for a magnetic levitation train cable of this embodiment, the raw materials and the formula are shown in Table 1.
[0089] Preparation method:
[0090] (1) A thermoplastic polyurethane elastomer, a novel phosphorus-nitrogen flame retardant, a charring agent, a smoke suppressant, an antioxidant, a stabilizer, and a reinforcing filler are added to an internal mixer, and melt-blended at 185° C. and 50 rpm for 10 min; after cooling and drying, the mixture is placed in a twin-screw extruder for melt-blending and extrusion, and the processing temperatures from the feed port to the die port are 175° C., 175° C., 180° C., 180° C., 185° C., and 185° C., respectively; after cooling and drying, a blended masterbatch is obtained.
[0091] (2) Add the above-mentioned blended masterbatch, color masterbatch, antioxidant and mildewproof agent into a high-speed mixer and mix them at 3000 r / min for 15 min; place them in a twin-screw extruder for melt blending and extrusion, and the processing temperatures from the feed port to the die port are 175° C., 175° C., 180° C., 180° C., 185° C. and 185° C., respectively; after cooling and drying, a cross-linked masterbatch is obtained.
[0092] (3) placing the cross-linked masterbatch in a wire and cable extruder for melt extrusion, wherein the inlet temperature is 140°C, the first section is 140-150°C, the second section is 150-160°C, the third section is 160-170°C, the fourth section is 170-175°C, the fifth section is 175-180°C, and the outlet temperature is 185°C; coating the surface of the cable conductor core with a sheath; irradiating the coated core for 10 minutes under the conditions of a beam pressure of 1.8 MeV, a beam current of 40 mA, and an irradiation dose of 300 kGy to obtain a finished cable.
[0093] Example 5
[0094] The present embodiment is a sheath material for a maglev train cable, the raw materials and formula are shown in Table 1, and the preparation method is the same as that of Example 4.
[0095] Example 6
[0096] The present embodiment is a sheath material for a maglev train cable, the raw materials and formula are shown in Table 1, and the preparation method is the same as that of Example 4.
[0097] Comparative Example 1
[0098] A sheath material of this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as that of Example 4.
[0099] Comparative Example 2
[0100] A sheath material of this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as that of Example 4.
[0101] Comparative Example 3
[0102] A sheath material of this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as that of Example 4.
[0103] Comparative Example 4
[0104] A sheath material of this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as that of Example 4.
[0105] Comparative Example 5
[0106] A sheath material of this comparative example, raw materials and formula are shown in Table 1.
[0107] Preparation method:
[0108] (1) A thermoplastic polyurethane elastomer, a novel phosphorus-nitrogen flame retardant, a reinforcing filler, a stabilizer, a carbonizing agent, a smoke suppressant, a mildew preventer, an antioxidant, an anti-aging agent, and a masterbatch are added to an internal mixer in proportion, and melt-blended at 185° C. and 50 rpm for 10 min; after cooling and drying, the mixture is placed in a twin-screw extruder for melt-blending and extrusion, and the processing temperature from the feed port to the die port is 175° C., 175° C., 180° C., 180° C., 185° C., and 185° C., respectively, and a blended masterbatch is obtained after cooling and drying.
[0109] (2) placing the above blended masterbatch in a wire and cable extruder for melt extrusion, with an inlet temperature of 140°C, a first section of 140-150°C, a second section of 150-160°C, a third section of 160-170°C, a fourth section of 170-175°C, a fifth section of 175-180°C, and an outlet temperature of 185°C, and coating the surface of the cable conductor core with a sheath; irradiating the coated core for 10 min under the conditions of a beam pressure of 1.8 MeV, a beam current of 40 mA, and an irradiation dose of 300 kGy to obtain a finished cable.
[0110] The main performance indicators of the cable sheath materials prepared in the above embodiments and comparative examples are shown in Table 2.
[0111] Table 2 Performance test results of the embodiments and comparative examples
[0112]
[0113]
[0114]
[0115] From Table 2, we can see that:
[0116] Due to the addition of the novel phosphorus-nitrogen flame retardant of the present invention, the carbonization ability of the material is improved, heat and combustible gas can be effectively isolated, it is not easy to precipitate, the heat release rate and smoke generation rate are reduced, the fire performance index is improved, and efficient flame retardancy is achieved. In addition, the novel phosphorus-nitrogen flame retardant structure contains a large number of rigid primitives, which can effectively improve the mechanical properties of the material. The introduction of hydroxyl-rich pentaerythritol and trimethylolethane (carbonizing agent) not only promotes carbonization, cooperates with the flame retardant of the novel phosphorus-nitrogen flame retardant, but also combines with the isocyanate group in the novel phosphorus-nitrogen flame retardant and plays a role in regulating and controlling the interfacial compatibility, and improves the tensile strength and elongation at break of the cable sheath material. The addition of antifungal agents cuprous oxide and calcium phosphate directly and effectively prevents mildew, thereby achieving an excellent long-term stable antifungal effect, and broadens the application field of the cable sheath material in harsh and complex environments. The step-by-step blending is adopted, and the shearing action between different melt strength gradients leads to uniform dispersion of the filler, and finally obtains a cable sheath material with excellent comprehensive performance.
[0117] Compared with Example 5, Comparative Example 1 uses traditional hydroxides, DOPO and melamine as flame retardants, resulting in poor flame retardancy and mechanical properties of the material. A large number of mildew spots are caused by the lack of mildew inhibitors, which makes it difficult to meet the use requirements in harsh and complex environments. Compared with Example 5, Comparative Example 2 uses traditional hydroxides, DOPO and melamine as flame retardants, and introduces a carbonizing agent, which can form a uniform carbon layer while realizing the rapid diffusion and storage of heat inside the material, which helps to improve the flame retardancy and fire resistance of the material, but the overall performance is still poor. Compared with Example 5, Comparative Example 3 introduces a new type of phosphorus-nitrogen flame retardant, which can effectively improve the flame retardancy of the material, and the flame retardant structure contains a large number of rigid primitives, which can effectively improve the mechanical properties of the material. However, the phase change system is not introduced, resulting in poor overall performance of the material. Compared with Example 5, Comparative Example 4 introduces a large number of new phosphorus-nitrogen flame retardants and carbonizing agents, which makes it difficult to disperse the filler evenly, and then the flame retardant reduces the interaction between the flame retardant and the polymer matrix. In summary, the superiority of the design formula of the present invention is reflected.
[0118] Comparative Example 5 and Example 5 have the same formula but different preparation processes. Comparative Example 5 uses traditional one-step mixing, which results in poor filler dispersion and difficulty in constructing a uniform and dense refractory layer, reflecting the superiority of the preparation process.
[0119] Combined with the test data analysis, it can be seen that the performance of high flame retardancy, high mechanical properties, and mildew resistance sheath materials for maglev train cables has been greatly improved. There are several reasons: (1) The new phosphorus nitrogen flame retardant contains DOPO flame retardant elements, triazine structure and a large number of benzene rings, which are easy to char, have excellent thermal stability, high flame retardant efficiency, and contain MDI structure, which makes it compatible with the matrix. The added content is small and does not precipitate, which can improve the comprehensive performance of the material. (2) The charring agent is a substance rich in oxygen elements such as trimethylolethane and pentaerythritol. While promoting charring, it combines with the isocyanate group in the new phosphorus nitrogen flame retardant to regulate the interface compatibility and improve the mechanical properties of the cable sheath material. (3) The introduction of inorganic mildew inhibitors such as cuprous oxide and calcium phosphate can effectively prevent mildew, thereby achieving an excellent long-term stable mildew resistance effect, which broadens the application field of the cable sheath material in harsh and complex environments. (4) Step-by-step blending is adopted to achieve uniform dispersion of fillers through the shearing effect between different melt strength gradients, and finally a cable sheath material with excellent comprehensive performance is obtained.
[0120] The present invention synthesizes a new type of phosphorus-nitrogen flame retardant with a specific structure, and uses trimethylolethane and pentaerythritol as carbonizing agents. When burning, it not only promotes carbonization, but also improves the carbonization ability of the material, can effectively isolate heat and combustible gases, is not easy to precipitate, reduces the heat release rate and smoke generation rate, improves the fire performance index, and achieves high-efficiency flame retardancy. In addition, it is combined with the isocyanate group in the new type of phosphorus-nitrogen flame retardant to play a role in regulating interface compatibility, and improves the tensile strength and elongation at break of the cable sheath material. In addition, the introduction of inorganic mildew inhibitors such as zinc ions, silver ions, and copper ion compounds can effectively prevent mildew, thereby achieving excellent long-term stable mildew-proof effects, and broadening the application field of the cable sheath material in harsh and complex environments. The material and related technologies are applied to cables for maglev trains with a speed of 620 kilometers per hour or more and cables for intelligent equipment serving in complex environments.
[0121] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A sheath material for a maglev train cable, characterized in that: The invention comprises the following raw materials in parts by weight: 100-150 parts of thermoplastic polyurethane elastomer, 30-50 parts of novel phosphorus-nitrogen flame retardant, 40-60 parts of reinforcing filler, 1.5-2.5 parts of stabilizer, 10-20 parts of carbonizing agent, 10-15 parts of smoke suppressant, 5-10 parts of mildewproof agent, 1.5-3 parts of antioxidant, 1-1.5 parts of anti-aging agent and 1-5 parts of masterbatch; The novel phosphorus-nitrogen flame retardant is a phenanthrene cyclotriazine cyanide DMMDI containing a 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide unit and a triazine structure, and the structural formula is shown in the following formula I: In Formula I, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms.
2. The sheath material for maglev train cables according to claim 1, characterized in that: The reinforcing filler is one or more of calcium carbonate, talc and kaolinite.
3. The sheath material for maglev train cables according to claim 1, characterized in that: The stabilizer is one or more of calcium stearate, barium stearate and zinc stearate.
4. The sheath material for maglev train cables according to claim 1, characterized in that: The carbon-forming agent is one or more of piperazine pyrophosphate, trimethylolethane, and pentaerythritol.
5. The sheath material for maglev train cables according to claim 1, characterized in that: The smoke suppressant is one or more of ammonium dimolybdate, calcium phosphomolybdate, hydroxide, and ammonium octamolybdate.
6. The sheath material for maglev train cables according to claim 1, characterized in that: The mildew inhibitor is one or more of zinc ions, silver ions, copper ion compounds, and calcium phosphate.
7. The sheath material for maglev train cables according to claim 1, characterized in that: The antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester, 2,2′-thiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N′-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, and tris[2,4-di-tert-butylphenyl]phosphite; the antioxidant is one or more of 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, N,N′-di(β-naphthyl)-p-phenylenediamine, N,N′-diphenyl-p-phenylenediamine, and N-phenyl-β-naphthylamine.
8. A method for manufacturing a sheath material for a maglev train cable according to any one of claims 1 to 7, characterized in that: Thermoplastic polyurethane elastomer, novel phosphorus-nitrogen flame retardant, carbonizing agent, smoke suppressant, antioxidant, stabilizer and reinforcing filler are added to an internal mixer for melt blending; after cooling and drying, the mixture is placed in a twin-screw extruder for melt blending and extrusion; after cooling and drying, a blended masterbatch is obtained; the blended masterbatch is added to a high-speed mixer for mixing with a color masterbatch, an antioxidant and a mildewproof agent; then, the mixture is placed in a twin-screw extruder for melt blending and extrusion; after cooling and drying, a cross-linked masterbatch is obtained; The cross-linked masterbatch is placed in a wire and cable extruder for melt extrusion to obtain a cross-linked cable; The cross-linked cable is irradiated to obtain a finished cable product.
9. The method for manufacturing a sheath material for a maglev train cable according to claim 8, characterized in that: The invention also includes the steps of preparing the novel phosphorus-nitrogen flame retardant: Melamine, N,N-dimethylformamide and 4-dimethylaminopyridine catalyst are added to a three-necked flask, and heated and stirred under a nitrogen atmosphere to completely dissolve them; p-olefin benzene carboxylic acid is then dissolved in N,N-dimethylformamide, added dropwise to the three-necked flask, and heated and stirred until the reaction is completed; after the reaction is completed, the reaction mixture is poured into excess deionized water to precipitate to obtain an intermediate product, which is then washed, rotary evaporated, and dried to obtain a triazine structure compound MCO represented by formula II: In formula II, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms; DOPO, 4,4′-methylenebis(phenyl isocyanate) and toluene are added to a three-necked flask and heated and stirred to completely dissolve, and then the triazine structure compound MCO is added, and heated and stirred until the reaction is completed; after the reaction is completed, the mixture is cooled to room temperature, filtered, washed and dried to obtain a novel phosphorus-nitrogen flame retardant DMMDI shown in Formula I: In Formula I, R1 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms, and R2 is an aliphatic substituent or an aromatic substituent having 0 to 6 carbon atoms.
10. An application of the sheath material for a maglev train cable as claimed in any one of claims 1 to 7, characterized in that: The material is used in cables for maglev trains with a speed of 620 kilometers per hour or above and cables for intelligent equipment serving in complex environments.
Citation Information
Cited By
High-strength flame-retardant PC / ABS alloy and preparation method thereof
CN120098426A