Halogen-free flame-retardant polyamide composition and preparation method thereof

Halogen-free flame-retardant polyamide composition is prepared by using long-carbon chain polyamide, melamine cyanurate salt, polyphosphate, amino silicone oil and SMA resin in the polyamide pipeline material, and the prior art has been solved The problem of insufficient flame retardant performance of polyamide pipeline materials has achieved the improvement of low-temperature toughness and hydrolysis resistance, and achieved the flame retardant performance of V0 level.

CN118931176AActive Publication Date: 2024-11-12ORINKO HIGH PERFORMANCE MATERIALS TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411174652.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

After the flame retardant modification of existing polyamide pipeline materials, the flame retardant performance can only reach V2 level, which cannot meet the needs of new energy vehicle cooling pipelines for high flexibility and hydrolysis resistance, especially in low temperature environments.

Method used

The formulation of raw materials such as long carbon chain polyamide, flame retardant melamine urea and melamine polyphosphate, plasticizer amino silicone oil, and chain extender styrene and maleic anhydride copolymerized by SMA resin, etc., is extruded through twin screws. The mechanism is prepared with halogen-free flame-retardant polyamide compositions, which combine antioxidants to improve the flame retardant properties and hydrolysis resistance of the material.

Benefits of technology

It has achieved new energy cooling pipe materials with good low-temperature toughness and good hydrolysis resistance, and its flame retardant performance reaches V0 level, providing better low-temperature toughness and flame retardant performance, and showing excellent durability in the application of new energy vehicle cooling water pipes sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010385130000011
    Figure BDA0005010385130000011
  • Figure BDA0005010385130000071
    Figure BDA0005010385130000071
  • Figure FDA0005010385120000011
    Figure FDA0005010385120000011
Patent Text Reader

Abstract

The invention discloses a halogen-free flame-retardant polyamide composition and a preparation method thereof. The halogen-free flame-retardant polyamide composition is prepared from the following components in parts by weight: 35-70 parts of long-carbon-chain polyamide resin, 5-32 parts of a polyamide elastomer, 5-15 parts of a flame retardant A, 5-20 parts of a flame retardant B, 2-20 parts of a plasticizer, 0.1-3 parts of a chain extender, 0.1-3 parts of an antioxidant and 0-3 parts of color master batch. Wherein the flame retardant A is melamine urea, and the flame retardant B is melamine polyphosphate. The long-chain nylon elastomer is used as the flexibilizer, the amino silicon oil with good flame retardance is used as the plasticizer, the high flexibility is provided, meanwhile, the amino silicon oil and the flame retardant generate a synergistic effect, and compared with a common polyamide plasticizer N-butylbenzenesulfonamide (BBSA), better flame retardance can be provided; the flame retardant is compounded by melamine cyanurate (MCA) and melamine polyphosphate, so that good halogen-free flame retardant performance is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer composite materials, in particular to a halogen-free flame-retardant polyamide composition and a preparation method thereof. Background Art

[0002] At present, with the rapid development of new energy vehicles, higher and higher requirements are put forward for the cooling pipes of new energy vehicles; from the original non-flame retardant pipes, there is a demand for flame retardant V0, hydrolysis-resistant, high-flexibility polyamide cooling pipe materials; at present, after the flame retardant modification of polyamide pipe materials, the flame retardancy can usually only reach V2 level, which greatly limits the application of the material. Summary of the invention

[0003] In view of this, the present invention provides a halogen-free flame-retardant polyamide composition and a preparation method thereof to solve the problems raised in the above-mentioned background technology. Through the formulation and process innovation of raw materials such as long carbon chain polyamide, flame retardant, chain extender, plasticizer, etc., the V0 flame retardant problem of the pipe is solved while ensuring the low temperature resistance and hydrolysis resistance of the pipe.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] In one aspect, the present invention discloses a halogen-free flame-retardant polyamide composition, which is prepared from the following components in parts by weight:

[0006]

[0007] Wherein, the flame retardant A is melamine urate, and the flame retardant B is melamine polyphosphate.

[0008] As a further embodiment of the present invention: the long carbon chain polyamide resin is at least one of polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 613, polyamide 614, polyamide 615, polyamide 616, polyamide 1010, polyamide 1012, polyamide 1013, polyamide 1014, polyamide 1015, polyamide 1016, polyamide 1210, polyamide 1212, polyamide 1213, polyamide 1214, polyamide 1215, and polyamide 1216.

[0009] As a further embodiment of the present invention: the polyamide elastomer is a polyetheramide having one of polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 613, polyamide 614, polyamide 615, polyamide 616, polyamide 1010, polyamide 1012, polyamide 1013, polyamide 1014, polyamide 1015, polyamide 1016, polyamide 1210, polyamide 1212, polyamide 1213, polyamide 1214, polyamide 1215, and polyamide 1216 as a hard segment and polyether as a soft segment.

[0010] As a further embodiment of the present invention: the plasticizer is amino silicone oil.

[0011] As a further solution of the present invention: the chain extender is SMA resin copolymerized by styrene and maleic anhydride.

[0012] As a further solution of the present invention: the antioxidant is at least one of antioxidant 1098, antioxidant 245, and antioxidant 168.

[0013] As a further embodiment of the present invention: the mass ratio of flame retardant A to flame retardant B is (1:3)-(3:1).

[0014] On the other hand, the present invention discloses a method for preparing the above-mentioned halogen-free flame-retardant polyamide composition, comprising the following steps:

[0015] Mixing: uniformly mix the long carbon chain polyamide resin, polyamide elastomer, flame retardant, chain extender, antioxidant and masterbatch to obtain material A;

[0016] Extrusion: Add material A into the main hopper of a twin-screw extruder, inject the plasticizer into the side hopper of the twin-screw extruder, and then obtain the halogen-free flame-retardant polyamide composition through strand drawing, pelletizing and drying.

[0017] As a further solution of the present invention: the temperature of one zone of the twin-screw extruder is 170-240°C, and the temperatures of other zones and the die are 225-280°C; the speed of the extruder is 50-1000r / min.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The present invention develops a new energy cooling pipe material with good low-temperature toughness, good hydrolysis resistance, and flame retardancy V0; long-chain nylon elastomer is used as a toughening agent to provide good low-temperature toughness;

[0020] (2) The present invention uses amino silicone oil with good flame retardancy as a plasticizer, which provides high flexibility and produces a synergistic effect with the flame retardant. Compared with the commonly used polyamide plasticizer N-butylbenzenesulfonamide BBSA, it can provide better flame retardant performance; the flame retardant is a compound of melamine cyanurate salt MCA and melamine polyphosphate, which can achieve good halogen-free flame retardant performance;

[0021] (3) The combined use of melamine ureate and melamine polyphosphate greatly improves the flame retardant properties. When melamine ureate is heated, it generates non-combustible gases, such as ammonia, which dilute the combustibles and oxygen produced by the polymer and reduce the concentration of combustible gases. The phosphoric acid substances produced by the decomposition of melamine polyphosphate at high temperature form a large amount of residual carbon on the surface of the material, effectively isolating oxygen and heat from entering the interior of the material and hindering the continued spread of flames. The combined use of the two can slow down the spread of fire in both the gas phase and the solid phase, and has a good synergistic effect.

[0022] (4) The present invention uses SMA resin copolymerized with styrene and maleic anhydride as a chain extender to increase the molecular weight of polyamide during modification, thereby increasing the viscosity of the composition and improving the hydrolysis resistance of the composition, making the composition particularly suitable for application in cooling water pipes of new energy vehicles. DETAILED DESCRIPTION

[0023] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0025] The specific information of the raw materials used in the following examples and comparative examples is as follows:

[0026] Polyamide 612, 235℃*2.16kg test, melt index 0.3g / 10min, produced by Huitong New Materials Co., Ltd.;

[0027] Polyamide 1012, 235℃*2.16kg test, melt index 3.2g / 10min, produced by Huitong New Materials Co., Ltd.;

[0028] Polyamide 1010, 235℃*2.16kg test, melt index 9.5g / 10min, produced by Huitong New Materials Co., Ltd.

[0029] Polyamide 614, 235℃*2.16kg test, melt index 5.7g / 10min, produced by Huitong New Materials Co., Ltd.;

[0030] Polyamide elastomer: PA12, PPBAPP 3533; PA12, PPBAPP 2533; PA12, PPBAPP 6333, all produced by Arkema;

[0031] Flame retardant A: MCA, BASF Melapur P MC 25; or, MCA, BASF Melapur P MC 50;

[0032] Flame retardant B: melamine polyphosphate JLS-PNA350 or melamine polyphosphate JLS-PNA, Hangzhou Jieersi;

[0033] Chain extenders: SMA PIRANP 9000, SMA PIRANP 3500, SMA PIRANP 1000, SMA PIRANP2000, all produced by POLYSCOPP of the Netherlands;

[0034] Antioxidant 1098, Antioxidant 168, Antioxidant 245, Antioxidant 1098, all produced by BASF;

[0035] Toughening agent: ShinPtsu KF-868 monoamine amino silicone oil, ShinPtsu KF-393 monoamine amino silicone oil, ShinPtsu KF-860 monoamine amino silicone oil produced by Shin-Etsu of Japan, and diamine amino silicone oil DY-N322 produced by Shandong Dayi Chemical;

[0036] All materials are commercially available conventional products.

[0037] It is to be understood that the above raw materials and reagents are only examples of some specific embodiments of the present invention, so that the technical solution of the present invention is clearer, and it does not mean that the present invention can only use the above reagents, and the specific scope in the claims shall prevail. In addition, the "parts" described in the examples and comparative examples, unless otherwise specified, refer to parts by weight.

[0038] Any range described in the present invention includes the end value and any numerical value between the end values ​​and any sub-range formed by the end value or any numerical value between the end values.

[0039] Example 1

[0040] Weigh 46.5 kg of polyamide 612, 20 kg of PA12 polyamide elastomer PPBAPP 3533, 6 kg of flame retardant MCAMMelapurP MC 25M, 13 kg of melamine polyphosphate JLS-PNA350, 2 kg of SMA resin (PIRANP9000), 0.5 kg of antioxidant 1098, 0.5 kg of antioxidant 168, and 1.5 kg of PA6 black masterbatch for standby use. Use a high-speed mixer to mix the above materials evenly, add them to the main weighing scale; add 10 kg of ShinPtsu KF-868 monoamine amino silicone oil to the liquid weighing scale, use a twin-screw extruder to granulate, dry the injection molded specimens, and test the mechanical properties and flame retardant properties.

[0041] Twin screw extruder parameters:

[0042] The temperature of zone 1 is 180℃, the temperature of zone 2 is 220℃, the temperature of zone 3 is 220℃, the temperature of zone 4 is 220℃, the temperature of zone 5 is 220℃, the temperature of zone 6 is 220℃, the temperature of zone 7 is 220℃, the temperature of zone 8 is 220℃, the temperature of zone 9 is 220℃, and the temperature of zone 10 is 230℃; the temperature of die head is 230℃; the speed of extruder is 200r / min.

[0043] Injection molding parameters: zone 1 temperature 180℃, zone 2 temperature 230℃, zone 3 temperature 230℃, die head temperature 230℃, nozzle temperature 230℃; mold temperature 50℃; plasticizing pressure 70MPa; back pressure 10MPa; injection pressure 60MPa; injection speed 50mm / s.

[0044] Example 2

[0045] Weigh 70 kg of polyamide 1012, 9 kg of PA12 polyamide elastomer PPBAPP 2533, 5 kg of flame retardant MCAMMelapurP MC 50M, 8.5 kg of melamine polyphosphate JLS-PNA, 0.5 kg of SMA resin (PIRANP3500), 3 kg of antioxidant 245, and 2 kg of antioxidant 168 for standby use. Use a high-speed mixer to mix the above materials evenly, add them to the main weighing scale; add 2 kg of ShinPtsu KF-393 monoamine amino silicone oil to the liquid weighing scale, use a twin-screw extruder to granulate, dry the injection molded strips, and test the mechanical properties and flame retardant properties.

[0046] The twin-screw extruder parameters and injection molding parameters are the same as in Example 1.

[0047] Example 3

[0048] Weigh 36.8 kg of polyamide 1010, 5 kg of PA12 polyamide elastomer PPBAPP 2533, 15 kg of flame retardant MCAMMelapurP MC 25M, 20 kg of melamine polyphosphate JLS-PNA370, 0.1 kg of SMA resin (PIRANP1000), 0.1 kg of antioxidant 1098, and 3 kg of PA6 black masterbatch for standby use. Use a high-speed mixer to mix the above materials evenly and add them to the main weighing scale; add 20 kg of diamine amino silicone oil DY-N322 to the liquid weighing scale, use a twin-screw extruder to granulate, dry the injection molded specimens, and test the mechanical properties and flame retardant properties.

[0049] The twin-screw extruder parameters and injection molding parameters are the same as in Example 1.

[0050] Example 4

[0051] Weigh 35 kg of polyamide 614, 32 kg of PA12 polyamide elastomer PPBAPP 6333, 14 kg of flame retardant MCAMMelapurP MC 50M, 5 kg of melamine polyphosphate JLS-PNA370, 3 kg of SMA resin (PIRANP2000), 1 kg of antioxidant 245, and 1 kg of antioxidant 168 for standby use. Use a high-speed mixer to mix the above materials evenly, add them to the main weighing scale; add 9 kg of ShinPtsu KF-860 monoamine amino silicone oil to the liquid weighing scale, use a twin-screw extruder to granulate, dry the injection molded specimens, and test the mechanical properties and flame retardant properties.

[0052] The twin-screw extruder parameters and injection molding parameters are the same as in Example 1.

[0053] Comparative Example 1

[0054] Weigh 46.5 kg of polyamide 612, 20 kg of PA12 polyamide elastomer PPBAPP 3533, 6 kg of flame retardant MCAMMelapurP MC 25M, 13 kg of melamine polyphosphate JLS-PNA350, 2 kg of SMA resin (PIRANP9000), 0.5 kg of antioxidant 1098, 0.5 kg of antioxidant 168, and 1.5 kg of PA6 black masterbatch for standby use. Use a high-speed mixer to mix the above materials evenly, add them to the main weighing scale; use a twin-screw extruder to granulate, dry the injection molded specimens, and test the mechanical properties and flame retardant properties.

[0055] The twin-screw extruder parameters and injection molding parameters are the same as in Example 1.

[0056] Comparative Example 2

[0057] Weigh 46.5 kg of polyamide 612, 20 kg of PA12 polyamide elastomer PPBAPP 3533, 6 kg of flame retardant MCAMMelapurP MC 25M, 13 kg of melamine polyphosphate JLS-PNA350, 2 kg of SMA resin (PIRANP9000), 0.5 kg of antioxidant 1098, 0.5 kg of antioxidant 168, and 1.5 kg of PA6 black masterbatch for standby use. Use a high-speed mixer to mix the above materials evenly, add them to the main weighing scale; add 10 kg of Proviron BBSA PROVIPLASPP 024 to the liquid weighing scale, use a twin-screw extruder to granulate, dry the injection molded specimens, and test the mechanical properties and flame retardant properties.

[0058] The twin-screw extruder parameters and injection molding parameters are the same as in Example 1.

[0059] Comparative Example 3

[0060] Weigh 46.5 kg of polyamide 612, 20 kg of PA12 polyamide elastomer PPBAPP 3533, 6 kg of flame retardant MCAMMelapurP MC 25M, 13 kg of melamine polyphosphate JLS-PNA350, 0.5 kg of antioxidant 1098, 0.5 kg of antioxidant 168, and 1.5 kg of PA6 black masterbatch for standby use. Use a high-speed mixer to mix the above materials evenly, add them to the main weighing scale; add 10 kg of monoamine amino silicone oil KF-868 to the liquid weighing scale, use a twin-screw extruder to granulate, dry the injection molded specimens, and test the mechanical properties and flame retardant properties.

[0061] The twin-screw extruder parameters and injection molding parameters are the same as in Example 1.

[0062] Comparative Example 4

[0063] Weigh 46.5 kg of polyamide 612, 6 kg of flame retardant MCAM Melapur P MC 25M, 13 kg of melamine polyphosphate JLS-PNA350, 2 kg of SMA resin (PIRANP 9000), 0.5 kg of antioxidant 1098, 0.5 kg of antioxidant 168, and 1.5 kg of PA6 black masterbatch for standby use. Use a high-speed mixer to mix the above materials evenly, add them to the main weighing scale; add 10 kg of monoamine amino silicone oil KF-868 to the liquid weighing scale, use a twin-screw extruder to granulate, dry the injection molded specimens, and test the mechanical properties and flame retardant properties.

[0064] The twin-screw extruder parameters and injection molding parameters are the same as in Example 1.

[0065] The mechanical properties and flame retardant properties of the materials prepared in Examples 1-4 and Comparative Examples 1-4 were tested, wherein the tensile test was conducted using an ISO 527 1A type bar, the simply supported beam impact test was conducted using an ISO 179 1eA bar, and the flame retardant bar was a UL94 1.6 mm bar. The test results are shown in Table 1:

[0066] Table 1

[0067]

[0068] Conclusion analysis:

[0069] 1. Compared with Example 1, in Example 1, amino silicone oil plasticizer was not added, and the notched impact strength at 23°C was 14.5 kJ / m 2 Down to 7.7 kJ / m 2 , flexibility decreased; flame retardancy dropped from V0 to V1, indicating that amino silicone oil has a synergistic effect on flame retardancy.

[0070] 2. In Comparative Example 2, BBSA plasticizer was used, and the flame retardant performance of the material decreased from UL94 1.6mm V0 to V2.

[0071] 3. In Comparative Example 3, no chain extender SMA resin was added, and the hydrolysis resistance of the material was seriously reduced. After hydrolysis for 1000 hours at 130°C and 50% ethylene glycol aqueous solution, the tensile strength decreased from 20.2 MPa to 12.1 MPa.

[0072] 4. In comparative example 4, no polyamide elastomer was added, and the -30°C notched impact strength was 5.6 kJ / m 2 Down to 1.8 kJ / m 2 , low temperature impact performance is poor.

[0073] Although this specification is described according to implementation modes, not every implementation mode includes only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0074] Therefore, the above description is only a preferred embodiment of the present application and is not intended to limit the scope of implementation of the present application; that is, all equivalent changes made according to the scope of the claims of the present application are within the protection scope of the claims of the present application.

Claims

1. A halogen-free flame-retardant polyamide composition, characterized in that: It is prepared from the following components by weight: Wherein, the flame retardant A is melamine urate, and the flame retardant B is melamine polyphosphate.

2. The halogen-free flame-retardant polyamide composition according to claim 1, characterized in that: The long carbon chain polyamide resin is at least one of polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 613, polyamide 614, polyamide 615, polyamide 616, polyamide 1010, polyamide 1012, polyamide 1013, polyamide 1014, polyamide 1015, polyamide 1016, polyamide 1210, polyamide 1212, polyamide 1213, polyamide 1214, polyamide 1215, and polyamide 1216.

3. The halogen-free flame-retardant polyamide composition according to claim 1, characterized in that: The polyamide elastomer is a polyetheramide with one of polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 613, polyamide 614, polyamide 615, polyamide 616, polyamide 1010, polyamide 1012, polyamide 1013, polyamide 1014, polyamide 1015, polyamide 1016, polyamide 1210, polyamide 1212, polyamide 1213, polyamide 1214, polyamide 1215, and polyamide 1216 as a hard segment and polyether as a soft segment.

4. The halogen-free flame-retardant polyamide composition according to claim 1, characterized in that: The plasticizer is amino silicone oil.

5. The halogen-free flame-retardant polyamide composition according to claim 1, characterized in that: The chain extender is SMA resin copolymerized with styrene and maleic anhydride.

6. The halogen-free flame-retardant polyamide composition according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1098, antioxidant 245, and antioxidant 168.

7. The halogen-free flame-retardant polyamide composition according to claim 1, characterized in that: The mass ratio of flame retardant A to flame retardant B is (1:3)-(3:1).

8. The method for preparing the halogen-free flame retardant polyamide composition according to any one of claims 1 to 6, characterized in that: The following steps are involved: Mixing: long carbon chain polyamide resin, polyamide elastomer, flame retardant, chain extender, antioxidant and masterbatch are uniformly mixed to obtain material A; Extrusion: Add material A into the main hopper of a twin-screw extruder, inject the plasticizer into the side hopper of the twin-screw extruder, and then obtain the halogen-free flame-retardant polyamide composition through strand drawing, pelletizing and drying.

9. The preparation method according to claim 7, characterized in that: The temperature of one zone of the twin-screw extruder is 170-240° C., and the temperatures of other zones and the die head are 225-280° C.; the rotation speed of the extruder is 50-1000 r / min.

Citation Information

Patent Citations

  • High flow non-spraying metallic silver polyamide composition and preparation method thereof

    CN108559258A

  • Easy-to-process anti-dripping low-smoke halogen-free flame-retardant polyolefin oxygen barrier material and preparation method thereof

    CN113956564A

  • Long-carbon-chain polyamide composition for battery sealing ring and preparation method of long-carbon-chain polyamide composition

    CN116102880A

  • Polyamide material and preparation method thereof

    CN117402490A

  • Plasticised and flameproof polyamide moulding compound and uses therefor

    WO2019122173A1

Cited By

  • Halogen-free flame-retardant long-chain nylon composite material and preparation method thereof

    CN119432056A

  • Halogen-free flame-retardant long-chain nylon composite material and preparation method thereof

    CN119432056B