Special copper-clad laminate insulating layer for mini backlight display and preparation method of special copper-clad laminate insulating layer

By using a combination of aminosilane polymer and hydroxy polyurethane acrylate polymer in the insulating layer, combining epoxy resin, amine-based curing agent, and thermally conductive filler, the existing insulating layer is solved by high brittleness under high temperature and high humidity conditions. The problem of high reliability and excellent thermal conductivity are achieved to prevent welding cracks.

CN118931204APending Publication Date: 2024-11-12TIANCHANG JINGFA ALUMINUM IND
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410973089.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The insulating layer of the existing metal-based copper clad foil laminate has a high elastic modulus and high brittleness under high temperature, high humidity and high pressure conditions, and cannot effectively absorb hot and cold impact stress, resulting in cracking of the pad and unable to meet the high reliability requirements.

Method used

Using a combination of aminosilane-containing polymer and hydroxyl-containing polyurethane acrylate polymer, the elastic modulus is reduced through flexible chain segments, combined with epoxy resin and amine-based curing agent to form a cross-linking network structure, increasing adhesion and heat resistance , and use aluminum nitride nanoparticles and graphene nanosheets as thermal fillers to form a continuous thermal conductivity path.

Benefits of technology

It significantly improves the stability and thermal conductivity of the insulating layer under high temperature and high humidity conditions, reduces the elastic modulus, prevents the occurrence of welding cracks, and improves welding reliability and comprehensive material performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004953787580000021
    Figure BDA0004953787580000021
  • Figure BDA0004953787580000071
    Figure BDA0004953787580000071
Patent Text Reader

Abstract

The invention relates to the technical field of new materials, and particularly provides a special copper-clad laminate insulating layer for mini backlight display and a preparation method thereof.The insulating layer comprises the following raw materials: an amino-containing silane polymer, a hydroxyl-containing urethane acrylate polymer, epoxy resin, phenoxy resin, an amine curing agent and a heat-conducting filler, the preparation method comprises the following steps: mixing raw materials with a solvent to prepare a resin glue solution with the solid content of 80%, uniformly coating the surface of a copper foil with the resin glue solution, drying at 160 DEG C for 5-10 minutes to obtain a semi-cured coating, and carrying out laminated combination and vacuum hot-pressing curing on a metal plate and the semi-cured coating to obtain the copper-clad laminate. According to the invention, the amino-containing silane polymer and the hydroxyl-containing polyurethane acrylate polymer gold are combined to obtain an insulating layer material with excellent thermal conductivity, heat resistance, peel strength, storage modulus, glass transition temperature, voltage resistance, insulation resistance and the like. The material is suitable for high-performance electronic components and high-temperature and high-pressure environments, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new materials, and in particular to an insulating layer of a copper-clad laminate special for mini backlight display and a preparation method thereof. Background Art

[0002] With the rapid development of electronic information technology, printed circuit boards (PCBs) continue to pursue high integration, high density, multi-functions, and small and thin shapes. Highly integrated and high-power-density electronic components will generate a lot of heat during operation. If they are not dissipated in a timely and effective manner, they may cause overheating and failure of the components. Therefore, thermally conductive metal-based copper-clad laminates (MCPCBs) have become an important material for solving heat dissipation problems and are widely used in general lighting, backlight devices, power control, and LED car headlights.

[0003] In the prior art, commonly used metal-based copper-clad laminates are usually made of an aluminum substrate or a copper substrate, a thermally conductive insulating adhesive layer (dielectric layer) and copper foil by hot pressing. The thermally conductive insulating adhesive layer is the key to determining the performance of MCPCB. At present, high heat-resistant resins and high filler content solutions are generally used to ensure the heat resistance stability, pressure resistance stability and heat dissipation of the insulation layer, but these insulation layers usually have a high elastic modulus and high brittleness, and cannot effectively absorb the stress generated by cold and hot shocks, which easily leads to cracking of the pads and cannot meet high reliability requirements.

[0004] In view of this, there is an urgent need to develop a dielectric layer material that has a low elastic modulus, excellent insulation performance under high temperature, high humidity and high pressure conditions, high thermal conductivity and excellent heat resistance, and good adhesion, so as to significantly improve welding reliability and meet the heat dissipation and insulation needs of high-power electronic components. Summary of the invention

[0005] In view of this, the present invention proposes a dielectric layer material that has a low elastic modulus, excellent insulation performance under high temperature, high humidity and high pressure conditions, high thermal conductivity and excellent heat resistance, and good adhesion, so as to significantly improve welding reliability and meet the heat dissipation and insulation requirements of high-power electronic components.

[0006] The technical solution of the present invention is implemented as follows: The present invention provides a copper-clad laminate insulation layer for mini backlight display, and the raw materials of the insulation layer are calculated by mass and include the following components:

[0007]

[0008] In the raw material scheme provided by the present invention, the aminosilane polymer has excellent flexibility and adhesion, and can maintain the stability of the material under high temperature and high humidity conditions. Its molecular skeleton is a flexible fatty chain structure, which helps to absorb and relieve the stress generated by the material during thermal expansion and contraction, and prevent the generation of welding cracks. The hydroxyl-containing polyurethane acrylate polymer contains flexible segments, which provide elasticity and chemical resistance to the material. The flexible segments in its molecular structure synergize with other polymers, so that the material has a lower elastic modulus and good flexibility after curing. The flexible segments of the aminosilane polymer and the hydroxyl-containing polyurethane acrylate polymer make the material have excellent flexibility after curing, reduce the elastic modulus, effectively absorb and relieve thermal stress, and prevent the generation of welding cracks.

[0009] In some embodiments, the aminosilane-containing polymer is one of amino-terminated polydimethylsiloxane and aminosilane-terminated polysiloxane, and / or; the weight average molecular weight of the amino-terminated polydimethylsiloxane is 5000-10000Da, and / or; the weight average molecular weight of the aminosilane-terminated polysiloxane is 4000-8000Da.

[0010] In some embodiments, the amino-terminated polydimethylsiloxane is available in the form of Xiameter OFX-0193 Fluid (Dow Corning); the aminosilane-terminated polysiloxane is available in the form of SLM-9190 (Gelest).

[0011] In some embodiments, the weight average molecular weight of the hydroxyl-containing polyurethane acrylate polymer is 1000-3500 Da.

[0012] In some embodiments, the epoxy resin is a combination of a bisphenol A epoxy resin and a bisphenol F epoxy resin.

[0013] In some embodiments, the mass ratio of bisphenol A epoxy resin to bisphenol F epoxy resin is 1:2.

[0014] Epoxy resin provides good adhesion, mechanical strength and electrical insulation. In the scheme, the combination of bisphenol A and bisphenol F epoxy resins can form a cross-linked network structure, improving the heat resistance and mechanical properties of the material. Phenoloxy resin has high heat resistance and excellent mechanical properties and can maintain stability in high temperature environments. During the curing process, phenoloxy resin works synergistically with other ingredients to form a strong cross-linked network structure.

[0015] In some embodiments, the phenolic resin is a phenolic epoxy resin.

[0016] In some embodiments, the amine curing agent is a combination of polyetheramine and ester cyclic amine, wherein the mass ratio of polyetheramine to ester cyclic amine is 1:2.

[0017] Amine curing agents can effectively cure epoxy resins to form a stable cross-linked network structure. The combination of polyetheramines and ester cyclic amines can provide excellent low temperature curing performance and high temperature stability.

[0018] In some embodiments, the thermally conductive filler is a combination of aluminum nitride nanoparticles and graphene nanosheets, wherein the mass ratio of the aluminum nitride nanoparticles to the graphene nanosheets is 3:2.

[0019] A high content of thermal conductive fillers (aluminum nitride nanoparticles and graphene nanosheets) can significantly improve the thermal conductivity of the material. Aluminum nitride nanoparticles and graphene nanosheets form a continuous thermal conduction path, dissipating heat quickly and effectively, and maintaining stable operation of components.

[0020] In some embodiments, the average particle size of the aluminum nitride nanoparticles is 20-50 nm, and the graphene nanosheets are single-layer or few-layer nanosheets with a sheet diameter of 1-5 μm.

[0021] In the second aspect, the present invention also provides a method for preparing an insulating layer of a copper-clad laminate dedicated to a mini backlight display, comprising the following steps: mixing the raw materials with a solvent to prepare a resin adhesive with a solid content of 80%, uniformly coating the resin adhesive on the surface of the copper foil, drying at 160°C for 5-10 minutes to obtain a semi-cured coating, stacking a metal plate and the semi-cured coating, and vacuum hot pressing and curing to obtain a copper-clad laminate.

[0022] The insulating layer is obtained by curing the adhesive layer in the copper-clad laminate prepared by the above preparation method.

[0023] The temperature of the vacuum hot pressing curing is 190°C and the pressure is 25kg / cm 2 , hot pressing time is 40min.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The raw materials of the insulating layer provided by the present invention use flexible segments of aminosilane polymers and hydroxyl-containing polyurethane acrylate polymers, which make the material have excellent flexibility after curing, reduce the elastic modulus, effectively absorb and relieve thermal stress, and prevent the generation of welding cracks. Compared with the prior art, it has better stability under high temperature and high humidity conditions. The hydroxyl-containing polyurethane acrylate polymer provides better elasticity and chemical resistance, which helps to absorb and relieve the stress generated by the material during thermal expansion and contraction, and prevent the generation of welding cracks. Aminosilane has excellent adhesion and can form strong bonds with inorganic and organic materials to ensure a firm bond between the insulating layer and the substrate and components. Polyurethane acrylate has excellent heat resistance and chemical stability, can maintain performance unchanged in high temperature environments, and improve the service life of the insulating layer. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.

[0028] Unless otherwise specified, the methods used in the following examples are all conventional methods. Unless otherwise specified, the materials, reagents and instruments used are all conventional materials, reagents and instruments in the art, and can be obtained by those skilled in the art through commercial channels.

[0029] When an amount, concentration or other value or parameter is expressed as a range, a preferred range or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range. In the present specification and claims, range definitions can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0030] The technical effects of the technical solution of the present application are described in detail below through examples and comparative examples.

[0031] The specific information of the raw materials involved in the embodiments is as follows:

[0032] A1: amino-terminated polydimethylsiloxane, model: Xiameter OFX-0193 Fluid (Dow Corning), weight average molecular weight 5000-10000 Da

[0033] A2: aminosilane-terminated polysiloxane, model: SLM-9190 (Gelest), weight average molecular weight 4000-8000 Da.

[0034] B1: hydroxyl-containing polyurethane acrylate polymer, model: CN996 (Sartomer), weight average molecular weight 2000-3000Da.

[0035] B2: hydroxyl-containing polyurethane acrylate polymer, model: EBECRYL 284 (Allnex), weight average molecular weight 1000-2000 Da.

[0036] B3: hydroxyl-containing polyurethane acrylate polymer, model: PHU 306-2 (Covestro), weight average molecular weight 1500-2500 Da.

[0037] B4: hydroxyl-containing polyurethane acrylate polymer, model: Laromer UA 9033 (BASF), weight average molecular weight 2500-3500 Da.

[0038] C1: bisphenol A type epoxy resin, model: Epon 828, (Hexion).

[0039] C2: bisphenol F type epoxy resin, model: LY 556, (Huntsman).

[0040] D1: phenolic epoxy resin, model: EPIKOTE 157, (Hexion).

[0041] E1: Polyetheramine, model: Jeffamine D-230.

[0042] E2: ester cyclic amine, isophorone diamine.

[0043] F1: aluminum nitride nanoparticles, average particle size: 20 nm.

[0044] F2: aluminum nitride nanoparticles, average particle size: 30 nm.

[0045] F3: Aluminum nitride nanoparticles, average particle size: 50 nm.

[0046] F4: graphene nanosheets, few layers, sheet diameter: 1μm.

[0047] F5: graphene nanosheets, few layers, sheet diameter: 3μm.

[0048] F6: graphene nanosheets, few layers, sheet diameter: 5μm.

[0049] Example 1

[0050] A copper-clad laminate insulation layer, the raw materials are composed by weight as follows:

[0051] The material proportions of each embodiment are shown in the following table:

[0052]

[0053]

[0054] Copper clad laminate preparation:

[0055] The raw materials and solvent are mixed to form a resin glue with a solid content of 80%. The resin glue is evenly coated on the surface of the copper foil and dried at 160°C for 5-10 minutes to obtain a semi-cured coating. The metal plate and the semi-cured coating are combined and vacuum hot-pressed for curing at a temperature of 190°C and a pressure of 25kg / cm 2 , the hot pressing time is 40 minutes, and a copper clad laminate is obtained.

[0056] The copper-clad laminates obtained in the above different embodiments were tested for performance in the following manner:

[0057] Thermal conductivity: Test the thermal conductivity of the plate according to the test method in standard ASTM-D5470;

[0058] Heat resistance (288℃ solder dip): Refer to the test conditions in IPC-TM-650 2.4.13 method to test the heat resistance of the board;

[0059] Peel strength: Refer to the test conditions in IPC-TM-650 2.4.8 method to test the peel strength of the board;

[0060] Storage modulus (elastic modulus): refer to the test conditions in IPC-TM-650 2.4.24.4 method to test the storage modulus of the dielectric layer at 25°C;

[0061] Glass transition temperature Tg: Refer to the test conditions in IPC-TM-650 2.4.24.4 method to test the Tg of the board;

[0062] Withstand voltage: According to the method in T / CPCA4105-2016, the withstand voltage performance of the dielectric layer is tested and the average value of the test at 5 points is taken;

[0063] Insulation resistance: Refer to the test conditions in IPC-TM-650 2.6.3 method to test the insulation resistance of the board.

[0064] The above performance test results are shown in the following table:

[0065]

[0066]

[0067] It can be seen from the data of the above embodiments that the insulating layer material of the present application has good comprehensive performance, among which embodiment 3 has a significant performance improvement compared with other data in embodiments 1-4, which is considered to be because a certain synergistic effect is formed between the aminosilane polymer A1 and the hydroxyl-containing polyurethane acrylate polymer B3, and the comparison between embodiment 5 and embodiment 3 shows that A2 and B3 form a better matching effect, and the data of embodiment 5 and embodiments 6-8 show that when the ratio of C1 to C2 in the epoxy resin is 1:2, it is optimal. It can be seen that the combination of C1 and C2 according to 1:2 has unexpected technical effects, while other ratios or C1 or C2 alone cannot achieve the technical effect of embodiment 5. Similarly, the data of comparative embodiment 5 and embodiments 9-10 show that only when the mass ratio of E1 to E2 is 1:2, there is a significant performance improvement. And the comparison between embodiment 5 and embodiments 12-22 shows that when F1 and F4 with a mass ratio of 3:2 are used, the technical effect is the best, while other ratios or other sizes of thermal conductive fillers cannot achieve its technical effect.

[0068] In summary, it can be seen that the present application provides a technical solution for an insulating layer using an aminosilane polymer and a hydroxyl polyurethane acrylate polymer. The insulating layer of this solution has good heat resistance, adhesion, insulation and flexibility, and based on the optimization of a series of parameters and materials, an insulating layer material with good comprehensive performance is obtained.

[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A copper-clad laminate insulation layer for mini backlight display, characterized in that: The raw materials of the insulating layer are calculated by weight and include the following components:

2. The copper-clad laminate insulating layer for mini backlight display as claimed in claim 1, characterized in that: The aminosilane-containing polymer is one of amino-terminated polydimethylsiloxane and aminosilane-terminated polysiloxane, and / or; the weight average molecular weight of the amino-terminated polydimethylsiloxane is 5000-10000Da, and / or; the weight average molecular weight of the aminosilane-terminated polysiloxane is 4000-8000Da.

3. The copper-clad laminate insulating layer for mini backlight display as claimed in claim 1, characterized in that: The weight average molecular weight of the hydroxyl-containing polyurethane acrylate polymer is 1000-3500 Da.

4. The copper-clad laminate insulating layer for mini backlight display as claimed in claim 1, characterized in that: The epoxy resin is a combination of bisphenol A epoxy resin and bisphenol F epoxy resin.

5. The copper-clad laminate insulating layer for mini backlight display as claimed in claim 1, characterized in that: The mass ratio of bisphenol A epoxy resin to bisphenol F epoxy resin is 1:

2.

6. The copper-clad laminate insulating layer for mini backlight display as claimed in claim 1, characterized in that: The phenolic resin is a phenolic epoxy resin.

7. The copper-clad laminate insulating layer for mini backlight display as claimed in claim 1, characterized in that: The amine curing agent is a combination of polyetheramine and ester cyclic amine, wherein the mass ratio of the polyetheramine to the ester cyclic amine is 1:

2.

8. The copper-clad laminate insulating layer for mini backlight display as claimed in claim 1, characterized in that: The thermal conductive filler is a combination of aluminum nitride nanoparticles and graphene nanosheets, wherein the mass ratio of the aluminum nitride nanoparticles to the graphene nanosheets is 3:

2.

9. The copper-clad laminate insulating layer for mini backlight display as claimed in claim 8, characterized in that: The average particle size of the aluminum nitride nanoparticles is 20-50 nm, and the graphene nanosheets are single-layer or few-layer nanosheets with a sheet diameter of 1-5 μm.

10. The method for preparing the insulating layer of the copper-clad laminate for mini backlight display according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing raw materials with a solvent to prepare a resin adhesive with a solid content of 80%, uniformly coating the resin adhesive on the surface of the copper foil, drying at 160° C. for 5-10 minutes to obtain a semi-cured coating, and stacking a metal plate and the semi-cured coating and performing vacuum hot pressing to cure the combination to obtain a copper-clad laminate.

Citation Information

Cited By

  • Resin composition and application thereof

    CN121592138A

  • High-wear-resistance oily filler-free adhesive coating and preparation method thereof

    CN122326084A