Lightweight plant fiber-based foamed high-strength high-buffering product and preparation process thereof

Through multi-biological enzyme treatment and molding foaming process, combined with isocyanate emulsion and gelatin, the problem of poor molding performance of plant fiber-based composite materials is solved, and high strength and buffering performance is improved, providing environmentally friendly high-performance products.

CN118931218APending Publication Date: 2024-11-12HUNAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411169709.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Plant fiber-based composite materials have problems of high density, low strength and uneven molding structure in molding processing, and traditional pretreatment methods cannot effectively improve their molding performance and bonding strength with other substances.

Method used

The plant fiber composition is treated with a combination of multi-biological enzymes, and the molding foaming process combines temperature regulation and foaming of isocyanate emulsion to achieve close bonding of large-pore foaming and fibers, and the skeleton is enhanced by gelatin, and the cell size and density are controlled.

Benefits of technology

The high strength, buffering performance and lightweight properties of plant fiber-based composite materials are achieved, the tensile strength and elongation of breaking are improved, the impact force is enhanced, and the environmentally friendly high-performance products are provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931218A_ABST
    Figure CN118931218A_ABST
Patent Text Reader

Abstract

The invention relates to a light plant fiber-based foaming product. The product is obtained by processing treated short plant fibers, bamboo fiber filaments, an isocyanate emulsion and a gelatin aqueous solution composition, the preparation process comprises the following steps: uniformly mixing the treated short plant fibers, the bamboo fiber filaments, the isocyanate emulsion and the gelatin solution at 60-70 DEG C to obtain a blank, cutting the blank into blocks, drying to control the moisture content to be 50-80%, adding the blank blocks into a molding press, maintaining the pressure for 2-3 minutes at 85-95 DEG C and 2.5-4.5 MPa, then quickly relieving the pressure, and preserving the heat for 3-5 minutes at 60-80 DEG C, so as to obtain a finished product. Naturally cooling to room temperature to obtain a product; the product has a large foam structure and low density, has excellent strength and buffering performance, and can be used as a buffering packaging material for replacing a plastic foam material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a plant fiber-based composite material and a lightweight high-strength and toughness product thereof, and in particular to a preparation method of a plant fiber-based composite molded material with uniform microporous structure, good strength and toughness. Background Art

[0002] Plant fiber is a natural renewable resource, widely found in agricultural and forestry resources and their processing waste, and is often not fully utilized and abandoned in nature as garbage, which also has a negative impact on the harmony of natural ecology, and may even cause serious fires due to improper treatment. High-value utilization of agricultural and forestry waste is an emerging strategic industry that the state has strongly encouraged to develop in recent years. However, in addition to a large amount of natural cellulose, this type of plant fiber also contains a large amount of hemicellulose, pectin, lignin and minerals, which will affect the performance of composite materials and limit the scope of use of the material.

[0003] Plant fibers are used as industrial or civilian materials, and they need to have good formability and strength during processing, but this is still a big problem. First of all, although natural plant fibers have high single fiber strength, they cannot be melted under normal conditions. The poor molding and processing performance causes uneven internal structure of the product and weak bonding between the fiber and other substances, which leads to a significant decrease in mechanical properties. Therefore, before molding, it is very necessary to pretreat the plant fibers to change their surface morphology, dimensional characteristics, surface chemical structure and molecular force, so as to improve their molding and processing performance and their bonding strength with other compound substances. Traditional pretreatment methods for plant fibers mainly include physical and chemical methods. Typical physical methods such as heat treatment, steam flash explosion, low-temperature plasma method, etc., only destroy the fiber structure through external force, improve the bonding force between the fiber and other substances and its own flowability. Compared with the above methods, bioenzyme treatment of plant fibers has more advantages. First, the bioenzyme treatment process is environmentally friendly and has low processing energy consumption; second, bioenzyme treatment has been proven to be effective in penetrating into the interior of plant fibers and regulating the fiber cell wall structure and surface chemical composition. However, how to find a better bio-enzyme treatment method to optimize the performance of plant fibers during processing and achieve product performance is still a major problem that needs to be solved.

[0004] In addition, for the processing and molding of plant fibers as raw materials, its performance is mainly determined by several aspects: first, the rheological processability of the raw materials, which will determine its distribution and defects in the molded body; second, the combination between the substances, which will determine the intrinsic strength of the material; third, in the lightweight process, the size and uniformity of the bubbles will also directly affect the mechanical properties. The fluidity of plant fiber-based composites directly determines the difficulty of their molding processing, and the uniform distribution of its raw materials directly affects the final performance of the material. Under normal circumstances, plant fibers are easy to agglomerate during high-temperature mixing processing, resulting in difficulties in melt flow, seriously affecting the processing performance of composite materials and causing performance deterioration. In order to improve this situation, it is particularly important to study the fluidity of plant fiber-based composites.

[0005] In order to solve this problem, the present invention develops a special plant fiber composition combined with bio-enzyme treatment, realizes the control of pores and the close combination of plant fibers through in-situ reaction combination and temperature-regulated foaming during the processing, and develops a molded foam material with better corresponding performance, providing a better option for environmentally friendly buffer materials. Summary of the invention

[0006] The purpose of the present invention is to overcome the defects of high density and low strength of plant fiber molding materials and to provide a special plant fiber composition which can achieve macroporous foaming while providing better strength and cushioning performance.

[0007] The objective of the present invention is achieved through the following technical solutions: A lightweight plant fiber-based foamed high-strength and high-cushioning product, the preparation process of which is as follows: The treated short plant staple fibers, bamboo fiber filaments, isocyanate emulsion and gelatin aqueous solution are uniformly mixed at 60-70° C. to obtain a blank, the blank is cut into pieces and dried to control the moisture content to between 50-80%, the blank is added into a molding machine and maintained at 85-95° C. and 2.5-4.5 MPa pressure for 2-3 minutes, then the pressure is released at a speed of 1.5-3 MPa / s, and the temperature is maintained at 60-80° C. for 3-5 minutes, and naturally cooled to room temperature to obtain a product; The invention is also characterized in that the mass ratio of each component is: Processed short plant fibers 100 Bamboo fiber filament 20-40 Isocyanate emulsion 15-30 Gelatin aqueous solution 20-40 Furthermore, the short plant fibers are derived from one or more of straw fibers, coconut shell fibers, sugarcane fibers, and wood fibers mixed in any proportion, preferably rice straw fibers or reed straw fibers.

[0008] Furthermore, the treated short plant fibers are plant fibers treated by a combination of multiple biological enzymes, and the specific process is: the plant fibers are crushed into 200-600 meshes, added into water to form a uniform slurry with a mass fraction of 30-50%, the slurry is put into a cellulase aqueous solution with a mass of 1-1.5 times that of the slurry and a mass concentration of 6-12%, after slowly stirring at 30°C-40°C for 2-4 hours, the temperature is raised to 80-90°C to inactivate the enzyme, and then the temperature is lowered to room temperature, and after coarse filtration, the slurry is put into a pectinase aqueous solution with a mass of 1-1.5 times that of the slurry and a mass concentration of 8-15%, after slowly stirring at 30°C-40°C for 2-4 hours, the temperature is raised to 80-90°C to inactivate the enzyme, and then the temperature is lowered to room temperature, and the treated plant fibers are obtained after filtration; the activities of cellulase and pectinase are between 2000-6000U / g.

[0009] Furthermore, the treated plant fibers have a diameter between 10-50 μm and an aspect ratio between 10-100.

[0010] Furthermore, the diameter of the bamboo fiber filament is between 100-300 μm, and the length is between 5-20 cm.

[0011] Furthermore, the bamboo fiber filaments are obtained by mechanically drawing bamboo, and the tensile strength of the single filaments is between 80-200 MPa.

[0012] Furthermore, the isocyanate emulsion is prepared by dissolving isocyanate in an organic solvent as an oily dispersed phase, adding the mixture into water containing a surfactant, and stirring at a high speed to form a stable oil / water emulsion; wherein the diameter of the dispersed isocyanate oil phase droplets is between 2-20 μm, and the volume of the dispersed oil phase droplets is between 35-50% of the emulsion.

[0013] Furthermore, the preparation method of the isocyanate emulsion is: adding isocyanate to a low-boiling point organic solvent, dissolving and stirring evenly, then adding to pure water containing a surfactant, and stirring at high speed to form an oil / water emulsion containing isocyanate oil phase particles; wherein the volume ratio of isocyanate to the low-boiling point organic solvent is between 1:2.5-4, and the amount of the surfactant used is between 2.5-4.5% of the water mass.

[0014] Furthermore, the isocyanate is one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, and dicyclohexylmethane diisocyanate; the low-boiling point organic solvent is an organic solvent with a boiling point below 85° C. at normal pressure and can dissolve isocyanate, including but not limited to ethyl acetate, hexane, and 1,2-methoxyhexane; the surfactant includes water / oil type surfactants such as span80, tween80, and tween20.

[0015] Furthermore, at the molding temperature, the low boiling point solvent encapsulating the isocyanate evaporates to generate gas for coordinated foaming.

[0016] Furthermore, the mass concentration of the gelatin aqueous solution is between 10-25%.

[0017] Furthermore, the gelatin may be industrial gelatin.

[0018] Furthermore, the cell size of the product is between 50-1000 μm.

[0019] Furthermore, the density of the product is between 0.91-1.12 kg / m 3 between.

[0020] Furthermore, after the prepared product is cut into standard specimens, it is tested according to GB / T 1040.1-2006 standard, and the tensile strength is between 18.5-28.5, and the elongation at break is between 69.7-148.5.

[0021] Furthermore, the prepared product is cut into a cuboid with a length*width*thickness of 10cm*10cm*1cm, and can withstand an impact force between 1200N and 3000N.

[0022] Furthermore, the technical advantages of the present invention are: (1) A special multi-enzyme combined treatment method is used to decompose fiber impurities such as fructose and hemicellulose, and fully destroy the fiber cell wall to achieve the combination of fiber, isocyanate emulsion and gelatin; (2) The isocyanate emulsion is added, and the low-boiling point organic solvent layer in the oil phase particles evaporates during the processing temperature and pressure relief process to act as a synergistic foaming agent, thereby exposing the isocyanate to react with the hydroxyl groups on the fiber surface to achieve the effect of cross-linking, enhancing and stabilizing the network; (3) Using water as the main foaming agent and organic solvent as the co-foaming agent, the foaming is regulated by the combined effects of temperature, pressure and pressure relief speed; (4) Add gelatin to fully soak the fibers and attach to the fiber skeleton to further strengthen the skeleton and stabilize the pores. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a scanning electron microscope image of the cross section of the product prepared in Example 1; Figure 2 This is a scanning electron microscope image of the cross section of the product prepared in Example 2. DETAILED DESCRIPTION

[0024] The exemplary implementation methods of the present invention will be described in detail below, but these implementation methods are for exemplary purposes only and the present invention is not limited thereto.

[0025] Example 1 A lightweight plant fiber-based foamed high-strength and high-cushioning product, the preparation process of which is as follows: The treated short plant fiber, bamboo fiber filament, isocyanate emulsion and gelatin aqueous solution are uniformly mixed at 65°C to obtain a blank, the blank is cut into pieces and dried to control the moisture content to 65%, the blank is added to a molding machine and maintained at 85°C and 3.2MPa pressure for 2.5 minutes, then the pressure is released at a speed of 2.5MPa / s, and the temperature is kept at 75°C for 4 minutes, and naturally cooled to room temperature to obtain a product; The invention is also characterized in that the mass ratio of each component is: Processed short plant fibers 100 Bamboo fiber filament 35 Isocyanate emulsion 26 Gelatin aqueous solution 35 The processed short plant fibers are reed straw fibers.

[0026] The treated short plant fiber is a plant fiber treated by a combination of multiple biological enzymes, and the specific process is: crushing reed straw into 300-500 meshes, adding it into water to prepare a uniform pulp with a mass fraction of 45%, putting the pulp into a cellulase aqueous solution with a mass fraction of 1.2 times that of the pulp and a mass concentration of 10%, slowly stirring at 35°C for 3 hours, heating it to 85°C to inactivate the enzyme, then cooling it to room temperature, and after coarse filtration, putting the pulp into a pectinase aqueous solution with a mass fraction of 1.4 times that of the pulp and a mass concentration of 12%, slowly stirring it at 35°C for 3 hours, heating it to 85°C to inactivate the enzyme, then cooling it to room temperature, and filtering to obtain the treated plant fiber; the activity of the cellulase is 3000U / g, and the activity of the pectinase is 5000U / g.

[0027] The treated short plant fibers have a diameter between 10 and 40 μm, and an aspect ratio between 10 and 100.

[0028] The diameter of the bamboo fiber filament is between 100-150 μm and the length is between 10-20 cm. The bamboo fiber filament is obtained by mechanically drawing bamboo.

[0029] The isocyanate emulsion is an oil / water emulsion formed by dissolving isophorone diisocyanate in ethyl acetate and then adding water containing 3.2% span80 by mass concentration; wherein the volume of dispersed oil phase droplets is 42% of the emulsion; The particle size of the isocyanate oil phase droplets is between 4 and 10 μm.

[0030] The gelatin is industrial gelatin, and the mass concentration of its aqueous solution is 14%.

[0031] like Figure 1As shown, the cell size of the product is between 50-100 μm.

[0032] The density of the product is 0.97 kg / m 3 .

[0033] The prepared product was cut into standard specimens and tested according to GB / T 1040.1-2006 standard, with a tensile strength of 27.8 MPa and an elongation at break of 127.8%.

[0034] The prepared product is cut into a cuboid with a length*width*thickness of 10cm*10cm*1cm, and can withstand an impact force of 2600N.

[0035] Example 2 A lightweight plant fiber-based foamed high-strength and high-cushioning product, the preparation process of which is as follows: The treated short plant fiber, bamboo fiber filament, isocyanate emulsion and gelatin aqueous solution are uniformly mixed at 70°C to obtain a blank, the blank is cut into pieces and dried to control the moisture content to 70%, the blank is added into a molding machine and maintained at 90°C and 4.0MPa pressure for 2 minutes, then the pressure is released at a speed of 3.2MPa / s, and the blank is kept at 78°C for 4 minutes, and naturally cooled to room temperature to obtain a product; The invention is also characterized in that the mass ratio of each component is: Processed short plant fibers 100 Bamboo fiber filament 22 Isocyanate Emulsion 20 Gelatin aqueous solution 38 The processed short plant fibers are wood fibers.

[0036] The treated short plant fibers are plant fibers treated by a combination of multiple biological enzymes, and the specific process is as follows: the wood fibers are crushed into 300-600 meshes, added into water to form a uniform pulp with a mass fraction of 40%, the pulp is put into a cellulase aqueous solution with a mass concentration of 11% and a mass time of 1.4 times the pulp, slowly stirred at 36°C for 3 hours, heated to 85°C to inactivate the enzyme, then cooled to room temperature, and after coarse filtration, the pulp is put into a pectinase aqueous solution with a mass concentration of 14% and a mass time of 1.2 times the pulp, slowly stirred at 36°C for 2.5 hours, heated to 85°C to inactivate the enzyme, then cooled to room temperature, and filtered to obtain the treated plant fibers; the activity of the cellulase is 5000U / g, and the activity of the pectinase is 4000U / g.

[0037] The treated short plant fibers have a diameter between 20 and 50 μm, and an aspect ratio between 20 and 80.

[0038] The diameter of the bamboo fiber filament is between 100-200 μm and the length is between 5-20 cm. The bamboo fiber filament is obtained by mechanically drawing bamboo.

[0039] The isocyanate emulsion is an oil / water emulsion formed by dissolving isophorone diisocyanate in ethyl acetate and then adding water containing 2.8% tween 20 by mass concentration; wherein the volume of the oil phase dispersed droplets is 38% of the emulsion.

[0040] The particle size of the isocyanate oil phase droplets is between 4 and 12 μm.

[0041] The gelatin is industrial gelatin, and the mass concentration of its aqueous solution is 18%.

[0042] like Figure 2 As shown, the cell size of the product is between 200-600 μm.

[0043] The density of the product is 1.04 kg / m 3 .

[0044] The prepared product was cut into standard specimens and tested according to GB / T 1040.1-2006 standard, with a tensile strength of 24.8 MPa and an elongation at break of 74.3%.

[0045] The prepared product is cut into a cuboid with a length*width*thickness of 10cm*10cm*1cm, and can withstand an impact force of 1600N.

[0046] Example 3 A lightweight plant fiber-based foamed high-strength and high-cushioning product, the preparation process of which is as follows: The treated short plant fiber, bamboo fiber filament, isocyanate emulsion and gelatin aqueous solution are uniformly mixed at 70°C to obtain a blank, the blank is cut into pieces and dried to control the moisture content to 72%, the blank is added to a molding machine and maintained at 92°C and 4.2MPa pressure for 2.5 minutes, then the pressure is released at a speed of 2.8MPa / s, and the temperature is kept at 76°C for 4.5 minutes, and naturally cooled to room temperature to obtain a product; The invention is also characterized in that the mass ratio of each component is: Processed short plant fibers 100 Bamboo fiber filament 25 Isocyanate emulsion 28 Gelatin aqueous solution 22 The processed short plant fibers are rice straw fibers.

[0047] The treated short plant fiber is a plant fiber treated by a combination of multiple biological enzymes. The specific process is: rice straw is crushed into 400-600 meshes, added into water to form a uniform slurry with a mass fraction of 45%, the slurry is put into a cellulase aqueous solution with a mass concentration of 10% and a mass time of 1.2 times the mass of the slurry, slowly stirred at 35°C for 3 hours, heated to 85°C to inactivate the enzyme, then cooled to room temperature, and after coarse filtration, the slurry is put into a pectinase aqueous solution with a mass concentration of 12% and a mass time of 1.4 times the mass of the slurry, slowly stirred at 38°C for 3.5 hours, heated to 85°C to inactivate the enzyme, then cooled to room temperature, and filtered to obtain the treated plant fiber; the activity of the cellulase is 4000U / g, and the activity of the pectinase is 5000U / g.

[0048] The treated short plant fibers have a diameter between 20 and 40 μm, and an aspect ratio between 30 and 100.

[0049] The diameter of the bamboo fiber filament is between 120-240 μm and the length is between 10-15 cm. The bamboo fiber filament is obtained by mechanically drawing bamboo.

[0050] The isocyanate emulsion is an oil / water emulsion formed by dissolving isophorone diisocyanate in hexane and then adding water containing 4% tween 80 by mass; wherein the volume of dispersed oil phase droplets is 40% of the emulsion.

[0051] The particle size of the isocyanate oil phase droplets is between 4 and 16 μm.

[0052] The gelatin is industrial gelatin, and the mass concentration of its aqueous solution is 20%.

[0053] The cell size of the product is between 50-500 μm.

[0054] The density of the product is 1.1 kg / m 3 .

[0055] The prepared product was cut into standard specimens and tested according to GB / T 1040.1-2006 standard, with a tensile strength of 22.6 MPa and an elongation at break of 128.9%.

[0056] The prepared product is cut into a cuboid with a length*width*thickness of 10cm*10cm*1cm, and can withstand an impact force of 2400N.

[0057] It can be seen from the above examples that the increase of bamboo fiber filaments is conducive to the improvement of strength and elongation at break, reflecting the role of the skeleton; the increase of isocyanate emulsion is conducive to the improvement of buffering performance, which indicates the improvement of the binding property of the treated plant fibers, and the increase of gelatin is conducive to the improvement of strength.

[0058] Comparative Example 1 Compared with Example 1, other formulas and processes are the same, except that bamboo fiber filaments are not added, and the properties obtained are as follows: The cell size of the product is between 50-800 μm.

[0059] The density of the product is 0.98 kg / m 3 .

[0060] The prepared product was cut into standard specimens and tested according to GB / T 1040.1-2006 standard, with a tensile strength of 14.8 MPa and an elongation at break of 63.5%.

[0061] The prepared product is cut into a cuboid with a length*width*thickness of 10cm*10cm*1cm, and can withstand an impact force of 850N.

[0062] This indicates that without adding bamboo fiber filaments, the strength and cushioning capacity of the material are significantly weakened, which significantly affects the bonding of the foamed material. At the same time, without adding bamboo fiber filaments, it is easy to cause the problem of unstable molding of the foamed product.

[0063] Comparative Example 2 Compared with Example 1, other formulas and processes are the same, only no isocyanate emulsion is added, and the properties obtained are as follows: The cell size of the product is between 100-1000 μm.

[0064] The density of the product is 1.17 kg / m 3 .

[0065] The prepared product was cut into standard specimens and tested according to GB / T 1040.1-2006 standard, with a tensile strength of 12.2 MPa and an elongation at break of 56.4%.

[0066] The prepared product is cut into a cuboid with a length*width*thickness of 10cm*10cm*1cm, and can withstand an impact force of 850N.

[0067] This indicates that not adding isocyanate emulsion reduces the amount of low-boiling organic solution added, reduces the amount of co-foaming agent, and reduces the number of small holes, but at the same time increases the density. In addition, due to the reduction of reactive components, the strength and cushioning properties of the material decrease.

[0068] Comparative Example 3 Compared with Example 1, other formulas and processes are the same, only without adding gelatin aqueous solution, the properties obtained are as follows: The cell size of the product is between 100-1000 μm.

[0069] The density of the product is 0.94 kg / m3 .

[0070] The prepared product was cut into standard specimens and tested according to GB / T 1040.1-2006 standard, with a tensile strength of 11.2 MPa and an elongation at break of 92.5%.

[0071] The prepared product is cut into a cuboid with a length*width*thickness of 10cm*10cm*1cm, and can withstand an impact force of 940N.

[0072] This indicates that not adding gelatin will also reduce the rigid network, resulting in an increase in the number of bubbles, a decrease in density, and a corresponding decrease in strength, but the toughness will be improved and the impact on cushioning will be smaller.

Claims

1. A lightweight plant fiber-based foamed high-strength high-cushioning product, the preparation process of which is: The treated short plant fiber, bamboo fiber filament, isocyanate emulsion and gelatin aqueous solution are uniformly mixed at 60-70° C. to obtain a blank, the blank is cut into pieces and dried to control the moisture content to between 50-80%, the blank is added into a molding machine and maintained at 85-95° C. and 2.5-4.5 MPa for 2-3 minutes, then the pressure is released at a speed of 1.5-3 MPa / s, and the temperature is maintained at 60-80° C. for 3-5 minutes, and naturally cooled to room temperature to obtain a product; The mass ratio of each component is: Processed short plant fibers 100 Bamboo fiber filament 20-40 Isocyanate emulsion 15-30 Gelatin aqueous solution 20-40 Its characteristics are also: The isocyanate emulsion is prepared by dissolving isocyanate in an organic solvent as an oily dispersed phase, adding the solution into water containing a surfactant, and stirring at high speed to form a stable oil / water emulsion; wherein the diameter of the dispersed isocyanate oil phase droplets is between 2-20 μm, and the volume of the dispersed oil phase droplets is between 35-50% of the emulsion.

2. A lightweight plant fiber-based foamed high-strength and high-cushioning product as claimed in claim 1, It is characterized in that The treated short plant fibers are plant fibers treated by multi-biological enzymes. The specific process is as follows: the plant fibers are crushed into 200-600 meshes, added into water to form a uniform pulp with a mass fraction of 30-50%, the pulp is put into a cellulase aqueous solution with a mass of 1-1.5 times that of the pulp and a mass concentration of 6-12%, and slowly stirred at 30°C-40°C for 2-4 hours, and then heated to 80-90°C to inactivate the enzyme, and then cooled to room temperature, and after coarse filtration, the pulp is put into a pectinase aqueous solution with a mass of 1-1.5 times that of the pulp and a mass concentration of 8-15%, and slowly stirred at 30°C-40°C for 2-4 hours, and then heated to 80-90°C to inactivate the enzyme, and then cooled to room temperature, and filtered to obtain the treated plant fibers; the activities of the cellulase and the pectinase are between 2000-6000U / g.

3. A lightweight plant fiber-based foamed high-strength and high-cushioning product as claimed in claim 1, It is characterized in that The diameter of the processed short plant fibers is between 10-50 μm, and the aspect ratio is between 10-100.

4. A lightweight plant fiber-based foamed high-strength and high-cushioning product as claimed in claim 1, It is characterized in that The processed short plant fibers are derived from one or more of straw fibers, coconut shell fibers, sugarcane fibers, and wood fibers, mixed in any proportion.

5. A lightweight plant fiber-based foamed high-strength and high-cushioning product as claimed in claim 1, It is characterized in that The diameter of the bamboo fiber filament is between 100-300 μm, and the length is between 5-20 cm.

6. A lightweight plant fiber-based foamed high-strength and high-cushioning product as claimed in claim 1, It is characterized in that The isocyanate emulsion is prepared by adding isocyanate to a low-boiling point organic solvent, dissolving and stirring the isocyanate, then adding the isocyanate to water containing a surfactant, and stirring at a high speed to form an oil / water emulsion containing isocyanate oil phase particles; wherein the volume ratio of the isocyanate to the low-boiling point organic solvent is between 1:2.5-1:4, and the amount of the surfactant used is between 2.5-4.5% of the mass of the water.

7. A lightweight plant fiber-based foamed high-strength and high-cushioning product as claimed in claim 1, It is characterized in that The isocyanate is one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, and dicyclohexylmethane diisocyanate; the low-boiling point organic solvent is an organic solvent with a boiling point lower than 85° C. at normal pressure and can dissolve isocyanate, including but not limited to ethyl acetate, hexane, and 1,2-methoxyhexane; the surfactant includes water / oil type surfactants such as span80, tween80, and tween20.

8. A lightweight plant fiber-based foamed high-strength and high-cushioning product as claimed in claim 1, It is characterized in that The mass concentration of the gelatin aqueous solution is between 10-25%.

9. A lightweight plant fiber-based foamed high-strength and high-cushioning product as claimed in claim 1, It is characterized in that The cell size of the product is between 50-1000 μm.