Gypsum putty powder production process
Through two-step calcination and grinding process optimization, combined with EDTA and sodium hexametaphosphate aid, the specific surface area and fineness of gypsum putty powder are improved, and the problem of insufficient environmental protection performance and decorative effect in the existing technology is solved, and a higher level of meet competitiveness and market demand.
Patent Information
- Application Number
- CN202411284458.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing gypsum putty powder has shortcomings in terms of environmental protection performance and decoration effect, and it is difficult to meet the market's demand for higher environmental protection performance and better decoration effect, especially in the trend of green decoration.
High whiteness phosphogypsum powder was obtained through a two-step calcination process, and grinding was performed using a mill to control the specific surface area and sieving rate. Add EDTA and sodium hexametaphosphate aids to optimize the grinding conditions to improve fineness and Whiteness meets market demand.
It has achieved high environmental protection performance and good decorative effect of gypsum putty powder, meets the market's technical and economic indicators for initial setting time, final setting time, whiteness and compressive strength, and improves the competitiveness and sustainable development capabilities of the product.
Abstract
Description
Technical Field
[0001] The invention relates to the field of gypsum putty powder processing, and in particular to a gypsum putty powder production process. Background Art
[0002] With the increasing awareness of environmental protection, green decoration will become the mainstream of the future decoration market. Decoration companies will pay more attention to the use of environmentally friendly materials and technologies to reduce pollution and waste during the decoration process. At the same time, the government will also introduce relevant policies to encourage and support the development of green decoration, especially the research and development and use of environmentally friendly materials. Among them, the environmental protection and comfort of the putty powder industry are favored by more and more people in decorative materials and environmentally friendly materials. Gypsum putty powder is a building material that can improve the quality of indoor environment. It has the advantages of stable performance, easy use, mildew resistance, good durability, high strength, strong adhesion, green environmental protection, low cost, etc. Compared with traditional putty, gypsum powder can replace part of the cementitious material and part of the filling material.
[0003] To this end, this project studies the gypsum putty powder process, aiming to improve the competitiveness of the green transformation of comprehensive utilization of phosphogypsum, and develop new putty products with higher environmental performance and better decorative effects. Customized services and green decoration will become the main development trends of the putty powder market. Therefore, it is necessary to adapt to market changes, seize development opportunities, and remain invincible in the future competition of phosphogypsum products to achieve sustainable development. Summary of the invention
[0004] The purpose of the present invention is to provide a gypsum putty powder production process research in view of the above-mentioned deficiencies. Through the control of specific process technical indicators, the specific surface area can be effectively increased, the fineness can be increased, the screening rate can be guaranteed, and a small amount of whiteness can be increased, thereby meeting market demand.
[0005] A gypsum putty powder production process of the present invention comprises the following steps: S1. calcining high-grade purified phosphogypsum through a two-step process to obtain decorative gypsum powder with a whiteness of 70%-75%; S2. Grind the decorative gypsum powder through a grinding machine. The 200-mesh sieving rate of the ground gypsum powder is controlled to be ≥95%, and the specific surface area is controlled to be 450-600m 2 / g, and obtain gypsum putty powder.
[0006] Preferably, the high-grade purified phosphogypsum in S1 is phosphogypsum with a purity of more than 90% and a whiteness of more than 50%.
[0007] Preferably, the crystal water content of the decorative gypsum powder calcined by the two-step method in S1 is controlled at 5.0%-6.0%, and the initial setting time is controlled at 6-7 minutes.
[0008] Preferably, the specific steps of calcination in the two-step method in S1 are as follows: the first step is to remove the attached water. At the hammer dryer, the high-temperature flue gas of 500-600 degrees generated by the hot air furnace is fully contacted with the phosphogypsum broken up by the hammer dryer to quickly remove 99% of the attached water. The dehydrated gypsum is induced to the dust removal flue gas separation and then enters the next step; the second step is to remove the crystallization water. In the boiling furnace tube, 200-degree steam is used to exchange heat with the gypsum outside the tube. The temperature in the furnace is controlled at 140-150 degrees to remove most of the crystallization water, and the remaining crystallization water is 5.0%-5.2%.
[0009] Preferably, during S2 grinding, the fan air volume of the grinding machine is controlled at 20370-25462m 3 / h, the fan pressure is controlled at 8330-8644pa.
[0010] Preferably, a gypsum powder grinding aid is added when the decorative gypsum powder in S2 is ground, and the gypsum powder grinding aid is a mixture of EDTA and sodium hexametaphosphate.
[0011] Preferably, the mass ratio of EDTA to sodium hexametaphosphate is 1:(0.8-1.0).
[0012] Preferably, the amount of the gypsum powder grinding aid added in S2 is 0.05%-0.10% of the total mass of the decorative gypsum powder.
[0013] The invention is based on key technical indicators as the innovation point. The technical and economic indicators achieved after production of this project are: Initial setting time: >6min Final setting time: <30min Whiteness:>70% 2h flexural strength: ≥2.5MPa 2h compressive strength: ≥5.0MPa.
[0014] Advantages of the invention: Through the control of process technical indicators, the specific surface area can be effectively increased, the fineness can be increased, the screening rate can be guaranteed, and a small amount of whiteness can be increased, thereby meeting market demand. DETAILED DESCRIPTION Example
[0015] A gypsum putty powder production process comprises the following steps: S1. calcining high-grade purified phosphogypsum through a two-step process to obtain decorative gypsum powder with a whiteness of 70%; S2. Grind the decorative gypsum powder through a grinding machine. The 200-mesh sieving rate of the ground gypsum powder is controlled to be ≥95%, and the specific surface area is controlled to be 450-550m 2 / g, and obtain gypsum putty powder.
[0016] S1 medium-to-high-grade purified phosphogypsum is phosphogypsum with a purity of more than 90% and a whiteness of more than 50%.
[0017] The crystal water content of the decorative gypsum powder calcined by the two-step method in S1 is controlled at 5.0%-5.4%, and the initial setting time is controlled at 6-7min.
[0018] The specific steps of the two-step calcination method in S1 are as follows: the first step is to remove the attached water. At the hammer dryer, the high-temperature flue gas of 500-600 degrees generated by the hot air furnace is fully contacted with the phosphogypsum broken up by the hammer dryer to quickly remove 99% of the attached water. The dehydrated gypsum is sent to the dust removal flue gas separation by induced air and then enters the next step; the second step is to remove the crystallization water. In the boiling furnace tube, 200-degree steam is used to exchange heat with the gypsum outside the tube. The temperature in the furnace is controlled at 140-150 degrees to remove most of the crystallization water, and the remaining crystallization water is 5.0%-5.2%.
[0019] During S2 grinding, the fan air volume of the grinding machine is controlled at 20370-22000m 3 / h, the fan pressure is controlled at 8330-8450Pa.
[0020] When the decorative gypsum powder in S2 is ground, a gypsum powder grinding aid is added, and the gypsum powder grinding aid is a mixture of EDTA and sodium hexametaphosphate.
[0021] The mass ratio of EDTA to sodium hexametaphosphate is 1:0.8.
[0022] The amount of gypsum powder grinding aid added in S2 is 0.05% of the total mass of decorative gypsum powder. Example
[0023] A gypsum putty powder production process of the present invention comprises the following steps: S1. calcining high-grade purified phosphogypsum through a two-step process to obtain decorative gypsum powder with a whiteness of 75%; S2. Grind the decorative gypsum powder through a grinding machine. The 200-mesh sieving rate of the ground gypsum powder is controlled to be ≥95%, and the specific surface area is controlled to be 500-600m 2 / g, and obtain gypsum putty powder.
[0024] S1 medium-to-high-grade purified phosphogypsum is phosphogypsum with a purity of more than 90% and a whiteness of more than 50%.
[0025] The crystal water content of the decorative gypsum powder calcined by the two-step method in S1 is controlled at 5.2%-5.6%, and the initial setting time is controlled at 6-7min.
[0026] The specific steps of the two-step calcination method in S1 are as follows: the first step is to remove the attached water. At the hammer dryer, the high-temperature flue gas of 500-600 degrees generated by the hot air furnace is fully contacted with the phosphogypsum broken up by the hammer dryer to quickly remove 99% of the attached water. The dehydrated gypsum is sent to the dust removal flue gas separation by induced air and then enters the next step; the second step is to remove the crystallization water. In the boiling furnace tube, 200-degree steam is used to exchange heat with the gypsum outside the tube. The temperature in the furnace is controlled at 140-150 degrees to remove most of the crystallization water, and the remaining crystallization water is 5.2%-6.0%.
[0027] During S2 grinding, the fan air volume of the grinding machine is controlled at 22000-25462m 3 / h, the fan pressure is controlled at 8450-8644pa.
[0028] When the decorative gypsum powder in S2 is ground, a gypsum powder grinding aid is added, and the gypsum powder grinding aid is a mixture of EDTA and sodium hexametaphosphate.
[0029] The mass ratio of EDTA to sodium hexametaphosphate is 1:1.0.
[0030] The amount of gypsum powder grinding aid added in S2 is 0.10% of the total mass of decorative gypsum powder. Example
[0031] A gypsum putty powder production process of the present invention comprises the following steps: S1. calcining high-grade purified phosphogypsum through a two-step process to obtain decorative gypsum powder with a whiteness of 73%; S2. Grind the decorative gypsum powder through a grinding machine. The 200-mesh sieving rate of the ground gypsum powder is controlled to be ≥95%, and the specific surface area is controlled to be 480-580m 2 / g, and obtain gypsum putty powder.
[0032] S1 medium-to-high-grade purified phosphogypsum is phosphogypsum with a purity of more than 90% and a whiteness of more than 50%.
[0033] The crystal water content of the decorative gypsum powder calcined by the two-step method in S1 is controlled at 5.4%-5.8%, and the initial setting time is controlled at 6-7min.
[0034] The specific steps of the two-step calcination method in S1 are as follows: the first step is to remove the attached water. At the hammer dryer, the high-temperature flue gas of 500-600 degrees generated by the hot air furnace is fully contacted with the phosphogypsum broken up by the hammer dryer to quickly remove 99% of the attached water. The dehydrated gypsum is sent to the dust removal flue gas separation by induced air and then enters the next step; the second step is to remove the crystallization water. In the boiling furnace tube, 200-degree steam is used to exchange heat with the gypsum outside the tube. The temperature in the furnace is controlled at 140-150 degrees to remove most of the crystallization water, and the remaining crystallization water is 5.5%-5.8%.
[0035] During S2 grinding, the fan air volume of the grinding machine is controlled at 22000-24000m 3 / h, the fan pressure is controlled at 8450-8550Pa.
[0036] When the decorative gypsum powder in S2 is ground, a gypsum powder grinding aid is added, and the gypsum powder grinding aid is a mixture of EDTA and sodium hexametaphosphate.
[0037] The mass ratio of EDTA to sodium hexametaphosphate is 1:0.9.
[0038] The amount of gypsum powder grinding aid added in S2 is 0.08% of the total mass of decorative gypsum powder.
[0039] The technical and economic indicators achieved by the gypsum putty powders of Examples 1-3 of the present invention all meet the following parameters: Initial setting time: >6min Final setting time: <30min Whiteness:>70% 2h flexural strength: ≥2.5MPa 2h compressive strength: ≥5.0MPa.
[0040] The above implementation cases are only for illustrating the technical solutions and features of the present invention, and their purpose is to enable people familiar with the technology to implement them better. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention are within the protection scope of the present invention, and those not described in detail are prior art.
Claims
1. A gypsum putty powder production process, characterized in that: The following steps are involved: S1. calcining high-grade purified phosphogypsum through a two-step process to obtain decorative gypsum powder with a whiteness of 70%-75%; S2. Grind the decorative gypsum powder through a grinding machine. The 200-mesh sieving rate of the ground gypsum powder is controlled to be ≥95%, and the specific surface area is controlled to be 450-600m 2 / g, and obtain gypsum putty powder.
2. A gypsum putty powder production process according to claim 1, characterized in that: S1 medium-to-high-grade purified phosphogypsum is phosphogypsum with a purity of more than 90% and a whiteness of more than 50%.
3. A gypsum putty powder production process according to claim 1, characterized in that: The crystal water content of the decorative gypsum powder calcined by the two-step method in S1 is controlled at 5.0%-6.0%, and the initial setting time is controlled at 6-7 minutes.
4. A gypsum putty powder production process according to claim 3, characterized in that: The specific steps of the two-step calcination method in S1 are as follows: the first step is to remove the attached water. At the hammer dryer, the high-temperature flue gas of 500-600 degrees generated by the hot air furnace is fully contacted with the phosphogypsum broken up by the hammer dryer to quickly remove 99% of the attached water. The dehydrated gypsum is sent to the dust removal flue gas separation by induced air and then enters the next step; the second step is to remove the crystallization water. In the boiling furnace tube, 200-degree steam is used to exchange heat with the gypsum outside the tube. The temperature in the furnace is controlled at 140-150 degrees to remove most of the crystallization water, and the remaining crystallization water is 5.0%-5.2%.
5. A gypsum putty powder production process according to claim 1, characterized in that: During S2 grinding, the fan air volume of the grinding machine is controlled at 20370-25462m 3 / h, the fan pressure is controlled at 8330-8644pa.
6. A gypsum putty powder production process according to claim 1, characterized in that: When the decorative gypsum powder in S2 is ground, a gypsum powder grinding aid is added, and the gypsum powder grinding aid is a mixture of EDTA and sodium hexametaphosphate.
7. A gypsum putty powder production process according to claim 6, characterized in that: The mass ratio of EDTA to sodium hexametaphosphate is 1:(0.8-1.0).
8. A gypsum putty powder production process according to claim 6, characterized in that: The amount of gypsum powder grinding aid added in S2 is 0.05%-0.10% of the total mass of decorative gypsum powder.
Citation Information
Patent Citations
Phosphogypsum deep purification method
CN111892314A
Method for preparing semi-hydrated gypsum powder by purifying ardealite and dynamically roasting
CN115448627A
Method for preparing architectural gypsum powder by using chemical gypsum as raw material through two steps method
CN1872763A