PE (polyethylene) film or PET (polyethylene terephthalate) aluminum laminated film surface ink-absorbing coating and preparation method thereof
By modifying the combination of porous silica and acrylic resin emulsion with cyclodextrin compounds, the problems of complex composition and insufficient adhesion in the prior art are solved, and efficient ink absorption performance and adhesion are achieved to meet the digital High adhesion and high definition requirements for printing.
Patent Information
- Application Number
- CN202411236732.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-04
AI Technical Summary
In the prior art, the composition system of the ink-absorbing coating on the surface of the PE film or PET aluminum-plated film is complex, and has high requirements for the dispersion performance and adhesion of ink-absorbing particles, making it difficult to meet the high adhesion and high definition requirements of digital printing.
Using cyclodextrin compound to modify porous silica as ink absorbing filler, and surface modification is performed by isocyanate-based silane coupling agent, combined with acrylic resin emulsion bonding material, improve the ink absorbing performance and adhesion of the coating, and simplify the component system .
It significantly improves the ink absorption performance and adhesion of the ink absorbing coating, meets the high adhesion and high-definition requirements of digital printing, and simplifies the coating preparation process.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of printing coatings, and in particular relates to an ink-absorbing coating on the surface of a PE film or a PET aluminized film and a preparation method thereof. Background Art
[0002] With the growing demand for personalized and small-batch packaging among consumers, digital printing is becoming more and more widely used. Unlike ordinary gravure printing, which requires customized and complex printing plates, digital printing does not require plate making. However, it has higher requirements on the ink absorbency of non-absorbent materials such as plastic films such as PE films or PET aluminized films. Therefore, ink-absorbing coatings applied on the surface of plastic films have emerged.
[0003] Water-based ink-absorbing coatings can quickly absorb ink or pigment, making the printed pattern clear and full, with higher and brighter color reproduction. This feature makes water-based ink-absorbing coatings perform well under high-resolution printing requirements and meet the strict requirements of modern printed products for color and clarity.
[0004] At present, due to its porous structure and good whiteness, SiO2 has been widely recognized in the market as an ink absorbent in an ink-absorbing coating. It not only has a fast absorption speed and a large absorption amount for water-based ink, but also can improve the controllability of the dot diameter and the dot roundness. At the same time, it can also reduce the scattering coefficient of the ink-absorbing layer and improve the image concentration. For example, CN 116396650 A discloses an ink-absorbing coating, which includes the following preparation raw materials in terms of mass percentage: 5-15% composite resin emulsion, 1-2% silicate, 15-30% nano silicon dioxide, 0.4-0.6% dispersant, 0.1-0.3% defoamer and the balance of water. The composite resin emulsion includes 10-20 parts of acrylate emulsion, 5-12 parts of water-based polyurethane emulsion and 2-8 parts of compatibilizer. The ink-absorbing coating can simultaneously improve the basic performance and ink absorption performance of the coating. However, the patented technology uses a composite resin of acrylate and waterborne polyurethane to improve the basic performance of the coating, which requires the use of a specific compatibilizer to improve compatibility and requires complex pretreatment of the nano-silica particles to improve their dispersion effect. The corresponding component system and preparation method are relatively complex.
[0005] Therefore, it is a technical problem that technicians in this field need to solve to provide an ink-absorbing coating with a simple component system, excellent coating performance, good adhesion to plastic films such as PE films or PET aluminum-coated films, excellent ink absorption performance, and excellent ink-absorbing particle dispersion performance. Summary of the invention
[0006] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide an ink-absorbing coating on the surface of a PE film or a PET aluminized film.
[0007] Another object of the present invention is to provide a method for preparing the ink-absorbing coating on the surface of the above-mentioned PE film or PET aluminized film.
[0008] The ink-absorbing coating of the present invention is mainly applied to the surface of PE and aluminum-plated PET substrates. The film surface coated with the ink-absorbing coating can adapt to digital inkjet printing. The digitally printed text and patterns have high clarity and good adhesion, and can also adapt to the requirements of post-processes such as lamination and bag making.
[0009] The purpose of the present invention is achieved through the following technical solutions:
[0010] An ink-absorbing coating for the surface of a PE film or a PET aluminized film, comprising the following components in percentage by mass:
[0011] Acrylic resin emulsion binder 60-80%, ink-absorbing filler 8-20%, viscosity regulator 1-5%, dispersant 1-4%, defoamer 0.1-0.3%, and the balance is water;
[0012] The ink-absorbing filler is a cyclodextrin compound-modified porous silica, which is prepared by the following method:
[0013] The cyclodextrin compound is heated and dissolved in an anhydrous solvent, and then an isocyanate silane coupling agent is added dropwise to carry out a heat-insulating stirring reaction. After the reaction is completed, porous silica powder is added and stirred to mix evenly, and water is added dropwise to continue the heat-insulating stirring reaction. The product is filtered, washed, and dried to obtain a cyclodextrin compound-modified porous silica.
[0014] Furthermore, the cyclodextrin compound is cyclodextrin (including α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin), hydroxyethyl cyclodextrin, hydroxypropyl cyclodextrin, carboxymethyl cyclodextrin, amino cyclodextrin; the amount of the cyclodextrin compound is 2-10% of the mass of the porous silica powder.
[0015] Furthermore, the anhydrous solvent is DMF (N,N-dimethylformamide) or DMAC (N,N-dimethylacetamide).
[0016] Furthermore, the isocyanate silane coupling agent is isocyanate propyl trimethoxy silane or isocyanate propyl triethoxy silane; the amount of the isocyanate silane coupling agent is 1 to 5% of the mass of the porous silica powder.
[0017] Furthermore, the porous silica powder is mesoporous (pore size between 2nm and 50nm) silica powder with a D50 particle size range of 2 to 5μm, which is a conventional raw material in the art.
[0018] Furthermore, the temperature for adding the isocyanate silane coupling agent, stirring and insulating the reaction, and the temperature for adding water, stirring and insulating the reaction, is 50 to 80° C., and the time is 2 to 6 hours.
[0019] Furthermore, the amount of water added is 3 to 5 times the molar amount of the isocyanate silane coupling agent. Adding a small amount of water can promote the hydrolysis of the coupling group to generate silanol, thereby promoting the surface modification reaction with the porous silica powder.
[0020] Furthermore, the acrylic resin emulsion binder can be a water-based acrylic resin emulsion prepared by copolymerizing a conventional (meth) acrylic acid ester monomer and a (meth) acrylic acid monomer. The acrylic acid ester monomer in the water-based acrylic resin emulsion provides good water resistance, and the acrylic acid monomer utilizes its polarity and hydrogen bonding effect to improve the adhesion to the plastic film and improve the bonding effect with the cyclodextrin compound modified porous silica ink-absorbing filler.
[0021] Preferably, the acrylic resin emulsion binder is prepared by the following method:
[0022] 1) dissolving isocyanoethyl (meth)acrylate in an anhydrous solvent, then adding a cyclodextrin compound to dissolve or disperse evenly, heating to 50-80° C. and stirring for reaction, and spray drying after the reaction is completed to obtain an acrylate-modified cyclodextrin compound crosslinking agent;
[0023] 2) Adding (meth)acrylate monomers, (meth)acrylic acid monomers, acrylate-modified cyclodextrin compound crosslinking agent and emulsifier into deionized water, stirring and emulsifying to obtain an emulsion; then heating to 60-90° C., adding initiator solution dropwise to carry out polymerization reaction, and obtaining an acrylic resin emulsion binder.
[0024] Furthermore, in step 1), the cyclodextrin compound is cyclodextrin (including α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin), hydroxyethyl cyclodextrin, hydroxypropyl cyclodextrin, carboxymethyl cyclodextrin, amino cyclodextrin; and the anhydrous solvent is DMF or DMAC.
[0025] Furthermore, in step 1), the molar ratio of isocyanoethyl (meth)acrylate to cyclodextrin compound added is 2 to 6:1.
[0026] Furthermore, the (meth)acrylate monomers in step 2) are methyl acrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate; the mass ratio of the (meth)acrylate monomers, (meth)acrylic acid monomers, and acrylate-modified cyclodextrin compound crosslinking agent added is 1:(0.2-0.8):(0.1-0.3).
[0027] Furthermore, the emulsifier in step 2) is sodium alkyl sulfonate, sodium alkylbenzene sulfonate, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether; the amount of the emulsifier added is 1% to 4% of the total mass of the (meth)acrylate monomer, (meth)acrylic acid monomer and acrylate-modified cyclodextrin compound crosslinker.
[0028] Furthermore, the initiator in step 2) is ammonium persulfate, sodium persulfate or potassium persulfate.
[0029] Furthermore, the viscosity regulator is ethanol or isopropanol; the dispersant is polyvinyl alcohol; and the defoaming agent is TEGO Foamex-825 defoaming agent.
[0030] The method for preparing the ink-absorbing coating on the surface of the PE film or PET aluminized film comprises the following preparation steps:
[0031] The acrylic resin emulsion binder is stirred and mixed evenly with the viscosity regulator, dispersant and water, and then the ink-absorbing filler is added and stirred and dispersed evenly, and finally the defoamer is added and mixed evenly, and the ink-absorbing coating on the surface of the PE film or PET aluminum-plated film is obtained after standing.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) The present invention uses cyclodextrin compound-modified porous silica as an ink-absorbing filler, and utilizes the dual adsorption effects of chemical adsorption of cyclodextrin compound and physical adsorption of porous silica to significantly improve the ink absorption performance of the ink-absorbing coating. At the same time, modifying porous silica with cyclodextrin compound can improve its binding effect with acrylic resin emulsion binder and improve the dispersion effect of ink-absorbing filler.
[0034] (2) The present invention further uses a cyclodextrin compound cross-linked acrylic resin emulsion as a binder, which can further improve the strength and water resistance of the coating. At the same time, the cyclodextrin compound cross-linking unit introduced can provide a large number of polar groups, which can significantly improve the adhesion to plastic films such as PE film or PET aluminum-plated film. Finally, the cyclodextrin compound cross-linked acrylic resin emulsion binder can further improve the bonding effect with the cyclodextrin compound modified porous silica ink-absorbing filler, thereby improving the comprehensive performance of the coating. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0036] Example 1
[0037] A method for preparing an ink-absorbing coating on the surface of a PE film or a PET aluminized film, comprising the following preparation steps:
[0038] (1) Preparation of ink-absorbing filler
[0039] Hydroxyethyl-β-cyclodextrin (average molecular substitution degree of 7) was heated and dissolved in anhydrous DMF solvent at 70°C, and then isocyanate propyl triethoxysilane coupling agent was added dropwise to carry out heat preservation and stirring reaction for 3 hours. After the reaction was completed, porous silica powder (mesoporous silica with a particle size range of 2 to 5 μm) was added and stirred and mixed evenly. The amount of hydroxyethyl-β-cyclodextrin was 6% of the mass of porous silica powder, and the amount of isocyanate propyl triethoxysilane was 3% of the mass of porous silica powder. Then, deionized water with a molar amount of 4 times that of isocyanate propyl triethoxysilane was added dropwise and the reaction was continued for 2 hours of heat preservation and stirring. The product was filtered, washed with deionized water and ethanol in turn, and vacuum dried to obtain hydroxyethyl-β-cyclodextrin modified porous silica ink absorbent filler.
[0040] (2) Preparation of acrylic resin emulsion binder
[0041] Butyl acrylate, methyl methacrylate, acrylic acid and emulsifier sodium dodecylbenzene sulfonate are added into deionized water in a mass ratio of 70:30:50:4, stirred and emulsified to obtain an emulsion; then the temperature is raised to 70°C, and an ammonium persulfate initiator solution with a monomer weight of 0.2% is added dropwise to carry out polymerization reaction for 4 hours to obtain an acrylic resin emulsion binder with a solid content of 46%.
[0042] (3) Preparation of ink-absorbing coating
[0043] Measured by weight percentage, 70% acrylic resin emulsion binder, 2% isopropyl alcohol, 2% polyvinyl alcohol dispersant and 10.8% deionized water are stirred and evenly mixed, then 15% ink-absorbing filler is added and stirred and dispersed evenly, and finally 0.2% TEGO Foamex-825 defoamer is added and mixed evenly, and after standing, an ink-absorbing coating on the surface of PE film or PET aluminum-plated film is obtained.
[0044] The adhesion fastness (according to GB / T13217.7-2023), water resistance (immersed in 48°C warm water for 48h, dried at 80°C and tested for adhesion fastness), ink absorbency (coated on the surface of PE film or PET aluminized film at 5g / m 2(Dry pulp) ink-absorbing coating, test ink absorption value according to GB 12911-91), stability (centrifuge at 3000r / min for 10min, observe whether precipitation or stratification occurs). The test results show that the adhesion strength on PE film or PET aluminized film printing substrates is 95%; the water resistance test results show that the adhesion strength on PE film printing substrates is 88%, and the adhesion strength on PET aluminized film printing substrates is 85%; the ink absorption test results show that the ink absorption value on PE film printing substrates is 39%, and the ink absorption value on PET aluminized film printing substrates is 40%; the stability test results show no precipitation or stratification.
[0045] Example 2
[0046] A method for preparing an ink-absorbing coating on the surface of a PE film or a PET aluminized film, comprising the following preparation steps:
[0047] (1) Preparation of ink-absorbing filler
[0048] Heat β-cyclodextrin and dissolve it in anhydrous DMF solvent at 70°C, then add isocyanate propyl triethoxysilane coupling agent and stir for 3 hours. After the reaction is completed, add porous silica powder (mesoporous silica with a particle size range of 2 to 5 μm) and stir to mix evenly. The amount of β-cyclodextrin is 2% of the mass of porous silica powder, and the amount of isocyanate propyl triethoxysilane is 1% of the mass of porous silica powder. Then add deionized water 6 times the molar amount of isocyanate propyl triethoxysilane and continue to stir for 2 hours. The product is filtered, washed with deionized water and ethanol in turn, and vacuum dried to obtain β-cyclodextrin modified porous silica ink absorbent filler.
[0049] (2) Preparation of acrylic resin emulsion binder
[0050] Butyl acrylate, ethyl methacrylate, methacrylic acid and emulsifier alkylphenol polyoxyethylene ether are added into deionized water in a mass ratio of 60:40:80:5, stirred and emulsified to obtain an emulsion; then the temperature is raised to 70°C, and an ammonium persulfate initiator solution with a monomer weight of 0.2% is added dropwise to carry out polymerization reaction for 4 hours to obtain an acrylic resin emulsion binder with a solid content of 45%.
[0051] (3) Preparation of ink-absorbing coating
[0052] 80% of acrylic resin emulsion binder, 2% of isopropyl alcohol, 2% of polyvinyl alcohol dispersant and 7.8% of deionized water were stirred and evenly mixed by weight percentage, and then 8% of ink-absorbing filler was added and stirred and dispersed evenly, and finally 0.2% of TEGO Foamex-825 defoamer was added and mixed evenly, and the ink-absorbing coating on the surface of PE film or PET aluminum-plated film was obtained after standing.
[0053] The ink-absorbing coating obtained in this embodiment was tested to have an adhesion fastness of 95% on a PE film printing substrate, and an adhesion fastness of 96% on a PET aluminized film printing substrate; the water resistance test results showed that the adhesion fastness on the PE film printing substrate was 84%, and the adhesion fastness on the PET aluminized film printing substrate was 83%; the ink absorbency test results showed that the ink absorption values on the PE film and PET aluminized film printing substrates were both 28%; the stability test results showed no precipitation or stratification.
[0054] Example 3
[0055] A method for preparing an ink-absorbing coating on the surface of a PE film or a PET aluminized film, comprising the following preparation steps:
[0056] (1) Preparation of ink-absorbing filler
[0057] Hydroxypropyl-β-cyclodextrin (average molecular substitution degree of 5.2) was heated and dissolved in anhydrous DMF solvent at 70°C, and then isocyanate propyl trimethoxysilane coupling agent was added dropwise to carry out heat preservation and stirring reaction for 3 hours. After the reaction was completed, porous silica powder (mesoporous silica with a particle size range of 2 to 5 μm) was added and stirred and mixed evenly. The amount of hydroxypropyl-β-cyclodextrin was 10% of the mass of porous silica powder, and the amount of isocyanate propyl trimethoxysilane was 5% of the mass of porous silica powder. Then deionized water with a molar amount of 3 times that of isocyanate propyl trimethoxysilane was added dropwise and the reaction was continued for 2 hours of heat preservation and stirring. The product was filtered, washed with deionized water and ethanol in turn, and vacuum dried to obtain hydroxypropyl-β-cyclodextrin modified porous silica ink absorbent filler.
[0058] (2) Preparation of acrylic resin emulsion binder
[0059] Butyl acrylate, methyl methacrylate, acrylic acid and emulsifier sodium dodecylbenzene sulfonate are added into deionized water in a mass ratio of 70:30:20:5, stirred and emulsified to obtain an emulsion; then the temperature is raised to 70°C, and an ammonium persulfate initiator solution with a monomer weight of 0.2% is added dropwise to carry out polymerization reaction for 4 hours to obtain an acrylic resin emulsion binder with a solid content of 48%.
[0060] (3) Preparation of ink-absorbing coating
[0061] Calculated by weight percentage, 60% acrylic resin emulsion binder, 2% isopropyl alcohol, 2% polyvinyl alcohol dispersant and 15.8% deionized water are stirred and evenly mixed, then 20% ink-absorbing filler is added and stirred and dispersed evenly, and finally 0.2% TEGO Foamex-825 defoamer is added and mixed evenly, and after standing, an ink-absorbing coating on the surface of PE film or PET aluminum-plated film is obtained.
[0062] The ink-absorbing coating obtained in this embodiment was tested to have an adhesion fastness of 93% on a PE film printing substrate, and an adhesion fastness of 94% on a PET aluminized film printing substrate; the water resistance test results showed that the adhesion fastness on the PE film printing substrate was 87%, and the adhesion fastness on the PET aluminized film printing substrate was 88%; the ink absorbency test results showed that the ink absorption value on the PE film printing substrate was 46%, and the ink absorption value on the PET aluminized film printing substrate was 49%; the stability test results showed no precipitation or stratification.
[0063] Example 4
[0064] A method for preparing an ink-absorbing coating on the surface of a PE film or a PET aluminized film, comprising the following preparation steps:
[0065] (1) The preparation of ink-absorbing filler is the same as that in Example 1.
[0066] (2) Preparation of acrylic resin emulsion binder
[0067] 1) Dissolve isocyanoethyl methacrylate in DMF solvent, then add hydroxyethyl-β-cyclodextrin (average molecular substitution degree is 7) and dissolve evenly, the molar ratio of isocyanoethyl methacrylate to hydroxyethyl-β-cyclodextrin is 2:1, heat to 70° C. and stir to react for 3 hours, spray dry after the reaction is completed, and obtain an acrylate-modified cyclodextrin compound crosslinking agent.
[0068] 2) Butyl acrylate, methyl methacrylate, acrylic acid, an acrylate-modified cyclodextrin compound crosslinker and an emulsifier sodium dodecylbenzene sulfonate are added to deionized water in a mass ratio of 70:30:50:30:4, stirred and emulsified to obtain an emulsion; then the temperature is raised to 70° C., and an ammonium persulfate initiator solution containing 0.2% of the total weight of the monomers is added dropwise to carry out polymerization reaction for 4 hours to obtain an acrylic resin emulsion binder with a solid content of 46%.
[0069] (3) The preparation of the ink-absorbing coating is the same as in Example 1.
[0070] The ink-absorbing coating obtained in this embodiment was tested to have an adhesion strength of 100% on PE film and PET aluminized film printing substrates; the water resistance test results showed that the adhesion strength on the PE film printing substrate was 95%, and the adhesion strength on the PET aluminized film printing substrate was 92%; the ink absorbency test results showed that the ink absorption value on the PE film printing substrate was 51%, and the ink absorption value on the PET aluminized film printing substrate was 52%; the stability test results showed no precipitation or stratification.
[0071] Example 5
[0072] A method for preparing an ink-absorbing coating on the surface of a PE film or a PET aluminized film, comprising the following preparation steps:
[0073] (1) The preparation of ink-absorbing filler is the same as that in Example 1.
[0074] (2) Preparation of acrylic resin emulsion binder
[0075] 1) Dissolve isocyanoethyl acrylate in DMF solvent, then add β-cyclodextrin to dissolve and disperse evenly, the molar ratio of isocyanoethyl methacrylate to β-cyclodextrin is 4:1, heat to 70° C. and stir to react for 3 hours, spray dry after the reaction is completed, and obtain an acrylate-modified cyclodextrin compound crosslinking agent.
[0076] 2) Butyl acrylate, methyl methacrylate, acrylic acid, acrylate-modified cyclodextrin compound crosslinker and emulsifier sodium dodecylbenzene sulfonate are added to deionized water in a mass ratio of 70:30:50:20:4, stirred and emulsified to obtain an emulsion; then the temperature is raised to 70° C., and an ammonium persulfate initiator solution with a total monomer weight of 0.2% is added dropwise to carry out polymerization reaction for 4 hours to obtain an acrylic resin emulsion binder with a solid content of 46%.
[0077] (3) The preparation of the ink-absorbing coating is the same as in Example 1.
[0078] The ink-absorbing coating obtained in this embodiment was tested to have an adhesion fastness of 100% on PE film and PET aluminized film printing substrates; the water resistance test results showed that the adhesion fastness on the PE film printing substrate was 96%, and the adhesion fastness on the PET aluminized film printing substrate was 94%; the ink absorbency test results showed that the ink absorption values on the PE film and PET aluminized film printing substrates were both 48%; the stability test results showed no precipitation or stratification.
[0079] Example 6
[0080] A method for preparing an ink-absorbing coating on the surface of a PE film or a PET aluminized film, comprising the following preparation steps:
[0081] (1) The preparation of ink-absorbing filler is the same as that in Example 1.
[0082] (2) Preparation of acrylic resin emulsion binder
[0083] 1) Dissolve isocyanoethyl methacrylate in DMF solvent, then add hydroxypropyl-β-cyclodextrin (average molecular substitution degree is 5.2) and dissolve evenly, the molar ratio of isocyanoethyl methacrylate to hydroxyethyl-β-cyclodextrin is 6:1, heat to 70° C. and stir to react for 3 hours, spray dry after the reaction is completed, and obtain an acrylate-modified cyclodextrin compound crosslinker.
[0084] 2) Butyl acrylate, methyl methacrylate, acrylic acid, acrylate-modified cyclodextrin compound crosslinker and emulsifier sodium dodecylbenzene sulfonate are added to deionized water in a mass ratio of 70:30:50:10:4, stirred and emulsified to obtain an emulsion; then the temperature is raised to 70° C., and an ammonium persulfate initiator solution with a total monomer weight of 0.2% is added dropwise to carry out polymerization reaction for 4 hours to obtain an acrylic resin emulsion binder with a solid content of 46%.
[0085] (3) The preparation of the ink-absorbing coating is the same as in Example 1.
[0086] The ink-absorbing coating obtained in this embodiment was tested to have an adhesion strength of 100% on PE film and PET aluminized film printing substrates; the water resistance test results showed that the adhesion strength on the PE film printing substrate was 94%, and the adhesion strength on the PET aluminized film printing substrate was 93%; the ink absorbency test results showed that the ink absorption value on the PE film printing substrate was 44%, and the ink absorption value on the PET aluminized film printing substrate was 45%; the stability test results showed no precipitation or stratification.
[0087] It can be seen from the comparison results of the above Examples 4 to 6 with Example 1 that the present invention can further significantly improve the adhesion and water resistance of the obtained ink-absorbing coating on the PE film and PET aluminum-plated film printing substrates by further introducing an acrylate-modified cyclodextrin compound cross-linking agent into the acrylic resin emulsion binder, and also has a significant effect on improving the ink absorption performance.
[0088] Comparative Example 1
[0089] A method for preparing an ink-absorbing coating on the surface of a PE film or a PET aluminum-plated film. Compared with Example 1, an equal amount of unmodified porous silica powder (mesoporous silica with a particle size range of 2 to 5 μm) is used to replace the hydroxyethyl-β-cyclodextrin modified porous silica ink-absorbing filler, and the rest is the same.
[0090] The ink-absorbing coating obtained in this comparative example was tested to have an adhesion fastness of 91% on a PE film printing substrate, and an adhesion fastness of 90% on a PET aluminized film printing substrate; the water resistance test results showed that the adhesion fastness on the PE film printing substrate was 81%, and the adhesion fastness on the PET aluminized film printing substrate was 79%; the ink absorbency test results showed that the ink absorption values on the PE film and PET aluminized film printing substrates were both 33%; the stability test results showed obvious micropowder precipitation.
[0091] It can be seen from the comparison results of comparative example 1 and embodiment 1 that the stability of the ink-absorbing coating can be significantly improved by using cyclodextrin compounds to modify the surface of the silica ink-absorbing filler. At the same time, the chemical adsorption characteristics of the cyclodextrin compounds can further synergistically improve the ink-absorbing effect of the coating. In addition, the large number of polar groups introduced by the cyclodextrin compounds and the hydrogen bonding effect with the acrylic acid units in the acrylic resin emulsion binder can further improve the adhesion and water resistance of the coating on plastic films such as PE films or PET aluminum-plated films.
[0092] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. An ink-absorbing coating on the surface of a PE film or a PET aluminized film, characterized in that: The following components are included in percentage by mass: Acrylic resin emulsion binder 60-80%, ink-absorbing filler 8-20%, viscosity regulator 1-5%, dispersant 1-4%, defoamer 0.1-0.3%, and the balance is water; The ink-absorbing filler is a cyclodextrin compound-modified porous silica, which is prepared by the following method: The cyclodextrin compound is heated and dissolved in an anhydrous solvent, and then an isocyanate silane coupling agent is added dropwise to carry out a heat-insulating stirring reaction. After the reaction is completed, porous silica powder is added and stirred to mix evenly, and water is added dropwise to continue the heat-insulating stirring reaction. The product is filtered, washed, and dried to obtain a cyclodextrin compound-modified porous silica.
2. The ink-absorbing coating on the surface of a PE film or aluminized PET film according to claim 1, characterized in that: The cyclodextrin compound is cyclodextrin, hydroxyethyl cyclodextrin, hydroxypropyl cyclodextrin, carboxymethyl cyclodextrin and amino cyclodextrin; the dosage of the cyclodextrin compound is 2-10% of the mass of porous silica micropowder; the anhydrous solvent is DMF and DMAC.
3. The ink-absorbing coating on the surface of a PE film or aluminized PET film according to claim 1, characterized in that: The isocyanate silane coupling agent is isocyanate propyl trimethoxy silane and isocyanate propyl triethoxy silane; the amount of the isocyanate silane coupling agent is 1-5% of the mass of the porous silica powder; the porous silica powder is mesoporous silica powder with a D50 particle size range of 2-5 μm.
4. The ink-absorbing coating on the surface of a PE film or aluminized PET film according to claim 1, characterized in that: The temperature for adding the isocyanate silane coupling agent and stirring the reaction and the time for adding water and stirring the reaction is 50-80° C. and 2-6 hours; the amount of water added is 3-5 times the molar amount of the isocyanate silane coupling agent.
5. The ink-absorbing coating on the surface of a PE film or aluminized PET film according to claim 1, characterized in that: The acrylic resin emulsion binder is prepared by the following method: 1) dissolving isocyanoethyl (meth)acrylate in an anhydrous solvent, then adding a cyclodextrin compound to dissolve or disperse evenly, heating to 50-80° C. and stirring for reaction, and spray drying after the reaction is completed to obtain an acrylate-modified cyclodextrin compound crosslinking agent; 2) Adding (meth)acrylate monomers, (meth)acrylic acid monomers, acrylate-modified cyclodextrin compound crosslinking agent and emulsifier into deionized water, stirring and emulsifying to obtain an emulsion; then heating to 60-90° C., adding initiator solution dropwise to carry out polymerization reaction, and obtaining an acrylic resin emulsion binder.
6. The ink-absorbing coating on the surface of a PE film or aluminized PET film according to claim 5, characterized in that: In step 1), the molar ratio of isocyanoethyl (meth)acrylate to cyclodextrin compound is 2 to 6:
1.
7. The ink-absorbing coating on the surface of a PE film or aluminized PET film according to claim 5, characterized in that: The (meth)acrylate monomers in step 2) are methyl acrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate; the mass ratio of the (meth)acrylate monomers, (meth)acrylic acid monomers, and acrylate-modified cyclodextrin compound crosslinking agent added is 1:(0.2-0.8):(0.1-0.3).
8. The ink-absorbing coating on the surface of a PE film or aluminized PET film according to claim 5, characterized in that: The emulsifier in step 2) is sodium alkyl sulfonate, sodium alkylbenzene sulfonate, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether; the amount of the emulsifier added is 1% to 4% of the total mass of the (meth)acrylate monomer, (meth)acrylic acid monomer and acrylate-modified cyclodextrin compound crosslinker; the initiator is ammonium persulfate, sodium persulfate, and potassium persulfate.
9. The ink-absorbing coating on the surface of a PE film or aluminized PET film according to claim 1, characterized in that: The viscosity regulator is ethanol or isopropanol; the dispersant is polyvinyl alcohol; and the defoaming agent is TEGO Foamex-825 defoaming agent.
10. The method for preparing the ink-absorbing coating on the surface of a PE film or aluminized PET film according to any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: The acrylic resin emulsion binder is stirred and mixed evenly with the viscosity regulator, dispersant and water, and then the ink-absorbing filler is added and stirred and dispersed evenly, and finally the defoamer is added and mixed evenly, and the ink-absorbing coating on the surface of the PE film or PET aluminum-plated film is obtained after standing.
Citation Information
Patent Citations
Ink-absorbing coating
CN116396650A
Water-based waterproof paint and preparation method and application thereof
CN103013245A
Cyclodextrin aqueous anticorrosive paint and preparation method thereof
CN105368258A
Matte, waterproof and ink-absorbing coating and preparation method thereof
CN106590223A
Method for preparing film print coating
CN109942859A