Preparation method of flame-retardant water-washable water-based acrylate resin coating with moderate compatibility

By introducing carbon-forming agent and porous carbon layer modifications into the washable coating, combined with gelatinization reaction of soluble starch, the coating melting and adhesion problems are solved, the flame retardancy and water solubility of the coating are improved, and the flame retardancy and water solubility of the coating are achieved. Efficient coating cleaning and improved drilling accuracy.

CN118931301AActive Publication Date: 2024-11-12HUIZHOU CAITIAN CHEM IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411419732.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-12
Estimated Expiration
2044-10-12

AI Technical Summary

Technical Problem

The existing washable coatings are melted due to poor heat resistance during the drilling process of PCB board, which affects the drilling accuracy and is difficult to clean, and the resin is not adhesion, which affects the performance and life of the circuit board.

Method used

The carbon-forming agent intermediate is used to conduct radical reaction with DOPO and 3,4-epoxy-1-butene, and combine the porous carbon layer modification and soluble starch to improve the flame retardant and water-soluble of acrylate resins and enhance the Its melt resistance and washability at high temperatures, and accelerates the reaction through gelatinized starch and alkaline environment to improve the melting temperature and water solubility of the resin.

Benefits of technology

It realizes rapid cleaning of coating films and improves drilling accuracy at high temperatures, reduces the number of resin film particles, improves the flame retardancy and washability of resins, and ensures the optimization of hole position accuracy and hole wall roughness of PCB plates .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a flame-retardant washable water-based acrylate resin coating with moderate compatibility, which comprises the following steps: adding water, an emulsifier and methacrylic acid, stirring to react for 60 minutes, adding a monomer A, a charring agent intermediate, DOPO and 3, 4-epoxy-1-butene, and emulsifying for 20-30 minutes; heating to 80-90 DEG C, dropwise adding an initiator, reacting for 1-2 hours, adding diethanol amine, and reacting for 1-2 hours to obtain a core-layer emulsion; the preparation method comprises the following steps: adding a monomer A and a monomer B into a reaction kettle, dropwise adding a monomer B and an initiator at the same time, keeping the temperature at 75-85 DEG C, stirring and reacting for 1.5 hours, adding DOPO, 3, 4-epoxy-1-butene and an initiator, reacting for 1 hour at 60-70 DEG C, cooling to 50 DEG C, adding an emulsifier B, reacting for 30 minutes, and adding ammonia water to adjust the pH value to 7-8, so as to obtain the flame-retardant washable water-based acrylate resin coating with moderate compatibility, and the obtained acrylate resin has good flame retardance and washability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a water-based acrylic resin coating, in particular to a method for preparing a flame-retardant, water-washable and moderately compatible water-based acrylic resin coating. Background Art

[0002] Temporary protective coatings are similar to general protective coatings, and can protect and remove dirt on the surface of the protected object. The difference is that the former has a short action time and mainly plays a protective role during processing, transportation or temporary storage. After the processing, transportation and storage process, the coating layer needs to be removed from the surface of the protected object. After the coating is removed, the original functions and properties of the protected object cannot be damaged or negatively affected. This kind of coating that plays a temporary protective role is also called removable coating or washable coating. Washable coatings can form a tightly structured film layer after being applied to the protected object, which can isolate the protected material from the outside world. At the same time, surface adsorption, adhesion and other effects during the film formation process can absorb dirt on the protected object.

[0003] Washable coatings are often removed from the surface of the protected object by soaking or washing with a specific solvent. The film must have a certain solubility in the solvent, which includes water, acid and alkali liquids, or specially formulated paint strippers. It is mainly used for glass and metal surface protection, or for vacuuming walls and floors and purifying the air.

[0004] PCB circuit boards are the cornerstone of electronic components. During the manufacturing process of PCB circuit boards, drilling accuracy is one of the core indicators for measuring PCB quality. Removable coatings are the key to industrial transformation and upgrading, and washable coatings are the key to affecting PCB drilling accuracy. Applying removable coatings on aluminum plates, and then attaching the aluminum plates with removable coatings to circuit boards (copper substrates, copper clad boards), and then drilling can improve the drilling accuracy of circuit boards. Coatings are consumables, and the PCB needs to be cleaned after the drilling operation is completed to remove the coating film. The water-washable coatings used in PCB processing on the market today generally have the following pain points: (a) PCB drilling requires drilling with the aluminum plate coating, but traditional water-washable coatings have poor heat resistance and cannot withstand the heat released during drilling operations, causing the coating film to partially or completely melt, affecting drilling accuracy; (b) Paint splashed during drilling is easy to adhere to the epoxy resin through-holes of the PCB and is difficult to handle. Residual paint is easy to cause moisture, mold, and corrosion of the circuit board, affecting the performance and life of the circuit board; (c) The resin adhesion between the PCB and the aluminum plate is not moderate, with poor adhesion, poor compatibility with the metal (aluminum plate), and difficulty in protection. The adhesion is too strong and it is also difficult to clean.

[0005] Jia Danfeng et al. prepared water-soluble acrylic resin by solution free radical polymerization method, using acrylic acid (AA), hydroxyethyl methacrylate (HEMA), acrylamide (AM) as functional monomers, butyl acrylate and methyl methacrylate as soft and hard monomers, azobisisobutyronitrile (AIBN) as initiator, and dimethylethanolamine as neutralizer. Then the water-soluble acrylic resin was compounded with the emulsion to prepare a water-based compounded resin for resin coating. The water-based compounded resin was compounded with fillers, water-soluble polymers and other additives to prepare a water-washable temporary protective coating. It was found that the adhesion of the film was level 2, and the demolding time at 50°C was 50s, showing a good water washing time. However, this technology did not consider the problem that the temporary coating film would adhere to the metal material when heated during use, causing the film to melt and be difficult to clean, and did not study core indicators such as PCB drilling accuracy.

[0006] Invention patent CN202210702763.5 involves using polyvinyl alcohol (PVA) resin as the main resin to improve the flexibility of the paint film; using polyether-modified acrylic resin as the modified resin to improve the adhesion of the paint on soft PVC and improve the water solubility of the PVA resin. At the same time, a small amount of acrylic-modified polyurethane (PUA) resin is used as the second modified resin to improve the bonding strength with soft PVC and resist cracking caused by deformation of the material. The invention also adds carboxylic acid-type propyl beet amphoteric surfactants to the coating, which has the dual effects of thickening and improving water washing residues, thereby accelerating the dissolution rate of the paint film when washed with water. Therefore, the coating provided by the invention has excellent flexibility, is not easy to crack, and has a good water washing effect. However, the patent involves cleaning of soft PVC, which is different from the use environment of the coatings used for aluminum plates and PCB epoxy resin boards, and does not involve the standard requirements for flame retardancy of acrylic esters.

[0007] Invention patent CN2015105882116 A kind of anti-carburizing coating that can be washed and removed after quenching is prepared by the following mass percentage components: 25~35% boric acid, 15~25% filler, 15~25% aluminum dihydrogen phosphate, 1~5% coloring pigment and 30~40% water. The invention also discloses the preparation method of the above anti-carburizing coating that can be washed and removed after quenching. The anti-carburizing coating can be removed by washing after carburizing heat treatment, thereby solving the problem that traditional anti-carburizing coating is difficult to peel off after carburizing heat treatment. Inorganic high temperature resistant materials are used as anti-carburizing agents in the formula of anti-carburizing coating. The anti-carburizing coating formed after the anti-carburizing agent is applied to the surface of the workpiece has good adhesion, and does not peel or flow at high temperature, and does not affect the carburizing atmosphere. The invention does not involve a film-forming agent with polyurethane resin as a film.

[0008] Invention patent 201910576686.1 relates to a glue-coated aluminum-based cover plate for PCB drilling and its preparation method, wherein the water-soluble composite polymer resin layer has moderate toughness and can play a guiding role during the falling process of the drill needle, thereby improving the drilling accuracy; at the same time, the hot-melt resin in the water-soluble composite polymer resin layer can lubricate the drill bit and cool the drill needle during drilling, thereby effectively improving the roughness of the hole wall, reducing wire winding, lowering the drill bit temperature, and extending the service life of the drill needle; in addition, the water-soluble composite polymer resin layer has good water solubility, is easy to handle after drilling, and is not easy to adhere to the holes in the PCB, thereby ensuring the drilling quality. The disadvantage of this resin is that it does not study whether the glue attached to the PCB hole during drilling can be cleaned, and does not emphasize the bonding of the film generated by the drill bit when heated.

[0009] Invention patent 201310504176.6 involves the following steps: (1) pre-processing the circuit board substrate, drilling through holes and copper deposition, board surface electroplating, outer layer circuit pattern transfer, pattern electroplating, etc.; 2) back drilling on PCB board 4 to detect whether the back drilling hole depth is qualified; 3) alkaline etching and photosensitive solder mask are performed on the drilled back drilling hole to finally obtain the finished product. The key points of its technical solution are: when back drilling, the drill belt coefficient used in the drilling through hole process should be modified according to the expansion and contraction data that appears in the process from drilling through holes to drilling back holes on PCB board 4, so as to keep the drill belt data consistent with the actual expansion and contraction; the drilling surface in the drilling through hole process is consistent with the drilling surface during back drilling; a layer of phenolic pad 6 is added on the top of PCB board 4; the depth accuracy and position accuracy of the existing back drilling holes on PCB board 4 can be effectively improved to ensure the integrity of the signal transmission on PCB board 4. The invention does not study the cleaning of the coating film and the bonding of the drill film and the adhesion of fragments.

[0010] In summary, the existing technology has not comprehensively studied the burning droplets of water-washable coatings applied in the aluminum cover, the heat tolerance (pkHHR, THR), the water washability of the film on the aluminum cover, the hole position accuracy of the PCB core, the hole wall roughness and the drill temperature, and the aperture melt and other indicators. The above indicators are the key to evaluating the performance of water-washable coatings, so research is imperative. Summary of the invention

[0011] The purpose of the present invention is to solve the problem that when drilling holes in the coating of a PCB board, the coating melts, which affects the drilling accuracy. At the same time, the coating melts due to heat, resulting in mucus of the film adhering to the hole of the PCB board, which solidifies and is difficult to remove. In view of the existing drawbacks, the present invention designs a flame-retardant, washable and moderately compatible water-based acrylic resin coating. First, in view of the thermal melting, the flame retardancy is improved to improve its index. A carbonizing agent intermediate is used in the core layer to react with DOPO and 3,4-epoxy-1-butene for free radical reaction, and the above substances are introduced into In the acrylic ester monomer chain segment, since both DOPO and p-hydroxybenzaldehyde have benzene ring rigid groups, their surface strength during the drilling process is moderate, and the accuracy will not be reduced due to high-speed movement during the drilling process, and the resin film will not be broken to form too many small particles and splash onto the PCB board, thereby reducing the number of resin film particles on the PCB board; secondly, the addition of 3,4-epoxy-1-butene will not make the resin film formed by DOPO and p-hydroxybenzaldehyde too hard and cause it to crack; using porous carbon layer modification , DOPO and 3,4-epoxy-1-butene participate in the shell free radical reaction, and the above substances are introduced into the acrylic resin segment to reduce the flammability of the acrylic resin; at the same time, the gelatinized starch also enhances the melting resistance of the PCB; then some hydroxyl groups of the soluble starch are used to react with the acyl chloride of benzoyl chloride to prevent the viscosity from increasing too much in the subsequent gelatinization; ammonium persulfate is used as an initiator to react acrylamide, hexadecyl dimethyl allyl ammonium chloride and N,N-methylenebisacrylamide with free radicals The solution reacts to form a soluble acrylic resin, and then the starch gelatinization is accelerated in an alkaline environment. The resulting gelatinized soluble starch has three functions: a. increasing the melting temperature of the acrylic resin, b. improving the water solubility of the acrylic resin, and c. increasing the swelling of the acrylic resin when heated and washed with water, so that it can be quickly peeled off from the epoxy resin PCB board and achieve moderate compatibility with the PCB board; in order to solve the water problem, hydrophilic acrylamide and hydroxyethyl acrylate are introduced into the shell layer to increase the water washability of the shell layer.

[0012] The preparation method of the flame-retardant, water-washable, moderately compatible water-based acrylic resin coating is prepared according to the following steps: (1) Preparation of core layer emulsion: add 600-800 g of water, 11-17 g of emulsifier A, and 24-41 g of methacrylic acid to a reaction container, mix and stir evenly, heat to 40-45°C, stir and react for 60 min, add monomer A, 10.2-13.4 g of carbonizing agent intermediate, 18.3-21.6 g of DOPO, and 2.1-6.3 g of 3,4-epoxy-1-butene, and emulsify for 20-30 min; heat to 65°C, pass reflux water, heat to 80-90°C, dropwise add 10-12 g of initiator, dropwise add for 1-1.5 h, react for 1-2 h, then add 3.15-8.4 g of diethanolamine, adjust the pH to 8, and react at 80-90°C for 1-2 h to obtain core layer emulsion; (2) To the whole core layer emulsion obtained in step (1), all monomers B and 8-12g of initiator are added dropwise at the same time for 1h, and the mixture is stirred at 75-85°C for 1.5h, and then 4.6-5.5g of porous carbon layer modifier, 4.1-4.3g of DOPO and 1.2-2.4g of 3,4-epoxy-1-butene, 2.1g of initiator and 1.1-2.3g of starch modifier are added, and the mixture is reacted at 60-70°C for 1h, and the temperature is lowered to 50°C, and 14-20g of emulsifier B is added, and the reaction time is 30min. Ammonia water is added to adjust the pH value to 7-8, and the flame-retardant, washable, and moderately compatible water-based acrylic resin coating is obtained; The monomer A is prepared by mixing 40-55g of ethyl acrylate, 28-48g of methyl methacrylate and 38-52g of hydroxyethyl acrylate; The monomer B is prepared by mixing 49-69 g of acrylamide, 12-54 g of methyl methacrylate and 55-92 g of hydroxyethyl acrylate.

[0013] The emulsifier A is prepared by mixing sodium dodecylbenzene sulfonate and AEO-9 in a mass ratio of 2:1; The preparation method of the carbon-forming agent intermediate is as follows: Add 6.1g of p-hydroxybenzaldehyde into a beaker, stir and dissolve with 100-150mL of ethanol, pour into a 250mL three-necked flask, stir at a speed of 250 r / min, heat to 50-60°C, slowly drop 1.5-1.8g of ethylenediamine diluted with 10mL of ethanol into the three-necked flask through a constant pressure dropping funnel, add dropwise for 30min, continue the reaction for 1-2.5h, stop heating, cool to room temperature, filter, and obtain a light yellow crude carbon-forming intermediate. Wash with ethanol three times, and vacuum dry at 60°C for 18-24h to obtain a light yellow carbon-forming intermediate powder, which is a carbon-forming agent intermediate.

[0014] The initiator is any one of ammonium persulfate and potassium persulfate; The preparation method of the porous carbon layer modified material is as follows: (1) Cut the vegetable tanned leather scraps into blocks with a length and width of 1 cm, place them in a vacuum tube furnace, heat them at 400 °C for 3-4 h in a nitrogen atmosphere for pre-carbonization, mix the obtained carbonized product with KOH in a mass ratio of 1:3, then add 300% water by weight to the above mixture, and stir at 40-50 °C for 18-22 h, then dry the product, and again carbonize and keep warm at 500-600 °C for 1-2 h under nitrogen protection, and finally dry it to obtain a porous carbon layer; (2) 0.5 g of porous carbon layer, 4.5-6.7 g of pyrrole, 100 mL of water, and 0.4-0.6 g of sodium p-toluenesulfonate were stirred at 50-60 °C for 2-4 h, and the product was dried. Then, 50 mL of DMF and 8.17-11.2 g of erythritol were added, and the pH was adjusted to 7.5. The mixture was stirred and reacted at 50-70 °C for 1-2 h. Then, 27.4-36.4 g of phosphorus trichloride was added, and the mixture was reacted at 30-40 °C for 1-2 h. Then, 12.5-15.3 g of myristic acid was added, and the mixture was reacted at 30-45 °C for 1-2 h. The product was dried to obtain a porous carbon layer modified product.

[0015] The preparation method of the starch modified material is as follows: add 1-1.2 g of benzoyl chloride and 15 mL of benzene to 4 g of soluble starch, stir and react at 30-40 ° C for 30-40 min, rotary evaporate at 40-50 ° C, and dry to obtain a starch reactant; then add 20 mL of 70 ° C deionized water to the starch reactant, stir for 30-40 min, add 0.03-0.05 g of ammonium persulfate at 50-60 ° C to obtain a pregelatinized soluble starch solution; then mix 5.8 g of acrylamide, 2.3 g of hexadecyl dimethyl allyl ammonium chloride and 2 g of N, N-methylene bisacrylamide, add to 10 mL of deionized water to dissolve, then slowly pour the solution into the pregelatinized soluble starch solution, adjust the pH of the soluble starch solution to 7.0 with a 1 mol / L NaOH aqueous solution, react for 15-30 min, the mixed solution becomes a gel state, and stir at 60-70 ° C for 2-3 h, then cut the gel into pieces with scissors, place it in an electric hot air drying oven at 90°C for 2-3 h, finally take it out and dry it for 24 h, crush it through an 18-mesh sieve, and the starch modification product is obtained; The emulsifier B is AEO-9.

[0016] The positive effects of the present invention are: (1) The present invention constructs a core-shell flame-retardant, water-washable and moderately compatible water-based acrylic resin. The core layer uses a relatively hard segment and the shell layer uses a soft segment. At a relatively high temperature, the film can be quickly removed from the hole of the PCB during cleaning. In the core layer, a carbonizing agent intermediate is used to react with DOPO and 3,4-epoxy-1-butene to carry out a free radical reaction, and the above substances are introduced into the acrylic monomer segment. Since DOPO and p-hydroxybenzaldehyde both have a benzene ring rigid group, the drilling process will not cause the accuracy to decrease due to the high-speed movement of the drilling process, and the resin film will not be broken to form too many small particles that splash onto the PCB board, thereby reducing the PCB The number of resin film particles on the board; secondly, the addition of 3,4-epoxy-1-butene will not make the resin film formed by DOPO and p-hydroxybenzaldehyde too hard and cause it to crack, and at a pH of 8, 3,4-epoxy-1-butene is ring-opened, and diethanolamine with strong hydrophilicity is introduced. The -NH of diethanolamine is used to open the ring with epoxy in an alkaline environment. On the one hand, nitrogen-containing elements with flame retardant effects are introduced into the acrylic resin chain. On the other hand, the introduced hydroxyl groups not only enhance the hydrophilicity of the resin core layer, but also dehydrate the hydroxyl groups into carbon during the heating process of the resin, thereby enhancing the resistance to droplets of the resin, reducing the resin film particles on the PCB board, and enhancing the water washability; (2) The present invention utilizes the aldehyde group of p-hydroxybenzaldehyde and the amino group of ethylenediamine to form a Schiff base through condensation of the aldehyde group and the imino group. This reaction occurs easily to generate an imine bond. Then, under the action of an initiator, the carbonizing agent intermediate, DOPO and 3,4-epoxy-1-butene undergo a free radical reaction, wherein the pH of DOPO reacts with the C=N or C=C double bond through an addition reaction to generate a core layer. Ethylenediamine provides nitrogen elements, and generates nitrogen and other flame-retardant gases during the combustion process, causing the carbon layer to expand. p-hydroxybenzaldehyde and DOPO provide carbon sources, and during combustion, a dense carbon layer is formed to cover the surface to isolate heat and oxygen. The phosphorus element in DOPO captures oxygen free radicals released by combustibles, reducing the possibility of combustion, thereby achieving a flame retardant effect.

[0017] (3) The present invention utilizes vegetable tanned leather scraps to be carbonized in a nitrogen atmosphere in an oxygen-isolated state, and uses KOH to increase its fluffiness, and then continues to carbonize to obtain a porous carbon layer. Pyrrole is dispersed in the porous carbon layer, and the phase change material erythritol is reacted with the NH bond of pyrrole, and the excess hydroxyl group reacts with phosphorus trichloride, and the excess phosphorus-chlorine bond reacts with myristic acid having a phase change, so that a large amount of phase change material is introduced into the porous carbon layer. When the material is heated, it can absorb part of the heat and delay the possibility of combustion. At the same time, a large amount of carbon is formed in the porous carbon layer, which reduces the possibility of combustion. Then, the porous carbon layer modifier, DOPO and 3,4-epoxy-1-butene are used to participate in the shell free radical reaction, and the above substances are introduced into the acrylic resin segment to reduce the flammability of the acrylic resin.

[0018] (4) The present invention utilizes part of the hydroxyl groups of soluble starch to react with the acyl chloride of benzoyl chloride, so that the viscosity of the soluble starch will not be excessively increased during the subsequent gelatinization; then the soluble starch is gelatinized in water, and the hydroxyl groups in the remaining starch are reacted with the amino group or the imino group, and ammonium persulfate or the like is used as an initiator to react acrylamide, hexadecyl dimethyl allyl ammonium chloride and N,N-methylene bisacrylamide in a free radical solution reaction to form a soluble acrylic resin; then the starch gelatinization is accelerated in an alkaline environment. The obtained gelatinized soluble starch has three functions: a) increasing the melting temperature of the acrylic resin; b) improving the water solubility of the acrylic resin; and c) increasing the swelling of the acrylic resin when heated and washed with water, so that the acrylic resin can be quickly peeled off from the epoxy resin PCB board to achieve moderate compatibility with the PCB board. DETAILED DESCRIPTION Embodiment 1

[0019] The preparation method of the flame-retardant, water-washable, moderately compatible water-based acrylic resin coating is prepared according to the following steps: (1) Preparation of core layer emulsion: add 600 g of water, 11 g of emulsifier A (mixed with sodium dodecylbenzene sulfonate and AEO-9 in a mass ratio of 2:1), and 24 g of methacrylic acid into a reaction container, mix and stir evenly, heat to 40°C, stir and react for 60 min, add monomer A, 10.2 g of carbonizing agent intermediate, 18.3 g of DOPO, and 2.1 g of 3,4-epoxy-1-butene, and emulsify for 20 min; heat to 65°C, pass reflux water, heat to 80°C, drop 10 g of ammonium persulfate initiator (dissolved in 50 g of water), drop for 1 h, react for 1 h, then add 3.15 g of diethanolamine, adjust the pH to 8, and react at 80°C for 1 h to obtain core layer emulsion; (2) To the whole core layer emulsion obtained in step (1), all monomers B and 8 g of ammonium persulfate initiator (dissolved in 40 g of water) were simultaneously added dropwise for 1 h, and the mixture was stirred at 75° C. for reaction for 1.5 h. Then, 4.6 g of porous carbon layer modifier, 4.1 g of DOPO, 1.2 g of 3,4-epoxy-1-butene, 2.1 g of ammonium persulfate initiator (dissolved in 4 g of water) and 1.1 g of starch modifier were added, and the mixture was reacted at 60° C. for 1 h. The mixture was cooled to 50° C., 14 g of emulsifier B (AEO-9) was added, and the reaction time was 30 min. Ammonia water was added to adjust the pH value to 7-8, and the flame-retardant, washable, and moderately compatible water-based acrylic resin coating was obtained. The monomer A is prepared by mixing 40 g of ethyl acrylate, 28 g of methyl methacrylate and 38 g of hydroxyethyl acrylate; The monomer B is prepared by mixing 49 g of acrylamide, 12 g of methyl methacrylate and 55 g of hydroxyethyl acrylate.

[0020] The preparation method of the carbon-forming agent intermediate is as follows: Add 6.1g of p-hydroxybenzaldehyde to a beaker, stir and dissolve it with 100mL of ethanol, and pour it into a 250mL three-necked flask with a stirring speed of 250 r / min. Heat to 50°C, slowly drop 1.5g of ethylenediamine diluted with 10mL of ethanol into the three-necked flask through a constant pressure dropping funnel, and add the dropwise addition time for 30min. Continue the reaction for 1h, stop heating, cool to room temperature, and filter to obtain a light yellow crude carbon-forming intermediate. Wash with ethanol 3 times, and vacuum dry at 60°C for 18h to obtain a light yellow carbon-forming intermediate powder, which is a carbon-forming agent intermediate.

[0021] The preparation method of the porous carbon layer modified material is as follows: (1) Cut the vegetable tanned leather scraps into blocks with a length and width of 1 cm, place them in a vacuum tube furnace, heat them at 400 °C for 3 h for pre-carbonization under a nitrogen atmosphere, mix the obtained carbonized product with KOH in a mass ratio of 1:3, then add 300% water by weight of the sample to the above mixture, and stir at 40 °C for 18 h, then dry the product, and carbonize it again at 500 °C for 1 h under nitrogen protection, and finally dry it to obtain a porous carbon layer; (2) 0.5 g of porous carbon layer, 4.5 g of pyrrole, 100 mL of water, and 0.46 g of sodium p-toluenesulfonate were stirred at 50 ° C for 2 h, the product was dried, and then 50 mL of DMF and 8.17 g of erythritol were added, the pH was adjusted to 7.5, and the reaction was stirred at 50 ° C for 1 h. Then 27.4 g of phosphorus trichloride was added and the reaction was carried out at 30 ° C for 1 h. Then 12.5 g of myristic acid was added and the reaction was carried out at 30 ° C for 1 h. The product was dried to obtain a porous carbon layer modified product.

[0022] The preparation method of the starch modified material is as follows: add 1 g of benzoyl chloride and 15 mL of benzene to 4 g of soluble starch, stir and react at 30 ° C for 30 minutes, rotary evaporate at 40 ° C, and dry to obtain a starch reactant; then add 20 mL of 70 ° C deionized water to the starch reactant, stir for 30 minutes, add 0.03 g of ammonium persulfate at 50 ° C to obtain a pregelatinized soluble starch solution; then mix 5.8 g of acrylamide, 2.3 g of hexadecyl dimethyl allyl ammonium chloride and 2 g of N, N-methylene bisacrylamide, add them to 10 mL of deionized water to dissolve, then slowly pour the solution into the pregelatinized soluble starch solution, adjust the pH of the soluble starch solution to 7.0 with a 1 mol / L NaOH aqueous solution, react for 15 minutes, the mixed solution becomes a gel state, stir and keep at 60 ° C for 2 hours, then cut the gel into pieces with scissors, place it in an electric hot air drying oven at 90 ° C for reaction for 2 hours, and finally take it out and dry it for 24 h. Grind and pass through an 18-mesh sieve to obtain the modified starch. Embodiment 2

[0023] The preparation method of the flame-retardant, water-washable, moderately compatible water-based acrylic resin coating is prepared according to the following steps: (1) Preparation of core layer emulsion: add 800 g of water, 17 g of emulsifier A (mixed with sodium dodecylbenzene sulfonate and AEO-9 in a mass ratio of 2:1), and 41 g of methacrylic acid into a reaction container, mix and stir evenly, heat to 45°C, stir and react for 60 min, add monomer A, 13.4 g of carbonizing agent intermediate, 21.6 g of DOPO, and 6.3 g of 3,4-epoxy-1-butene, and emulsify for 30 min; heat to 65°C and reflux water, heat to 90°C, add 12 g of potassium persulfate initiator (dissolved in 30 g of water), add for 1.5 h, react for 2 h, then add 8.4 g of diethanolamine, adjust the pH to 8, and react at 90°C for 2 h to obtain core layer emulsion; (2) To the whole core layer emulsion obtained in step (1), all monomers B and 12 g of potassium persulfate initiator (dissolved in 30 g of water) were simultaneously added dropwise for 1 h, and the mixture was stirred at 85° C. for 1.5 h. Then, 5.5 g of porous carbon layer modifier, 4.3 g of DOPO, 2.4 g of 3,4-epoxy-1-butene, 2.1 g of potassium persulfate initiator (dissolved in 10 g of water) and 2.3 g of starch modifier were added, and the mixture was reacted at 70° C. for 1 h. The mixture was cooled to 50° C., 17 g of emulsifier B (AEO-9) was added, and the reaction time was 30 min. Ammonia water was added to adjust the pH value to 7-8, and the flame-retardant, washable and moderately compatible water-based acrylic resin coating was obtained. The monomer A is prepared by mixing 55g of ethyl acrylate, 48g of methyl methacrylate and 52g of hydroxyethyl acrylate; The monomer B is prepared by mixing 69 g of acrylamide, 54 g of methyl methacrylate and 92 g of hydroxyethyl acrylate.

[0024] The preparation method of the carbon-forming agent intermediate is as follows: Add 6.1g of p-hydroxybenzaldehyde into a beaker, stir and dissolve with 150mL of ethanol, pour into a 250mL three-necked flask, stir at a speed of 250 r / min, heat to 60°C, slowly drop 1.8g of ethylenediamine diluted with 10mL of ethanol into the three-necked flask through a constant pressure dropping funnel, add dropwise for 30min, continue the reaction for 2.5h, stop heating, cool to room temperature, filter and obtain a light yellow crude carbon-forming intermediate, wash with ethanol three times, and vacuum dry at 60°C for 24h to obtain a light yellow carbon-forming intermediate powder, which is a carbon-forming agent intermediate.

[0025] The preparation method of the porous carbon layer modified material is as follows: (1) Cut the vegetable tanned leather scraps into blocks with a length and width of 1 cm, place them in a vacuum tube furnace, heat them at 400°C for 4 h in a nitrogen atmosphere for pre-carbonization, mix the obtained carbonized product with KOH in a mass ratio of 1:3, then add 300% water by weight to the mixture, and stir at 50°C for 22 h, then dry the product, and again carbonize and keep it at 600°C for 2 h under nitrogen protection, and finally dry it to obtain a porous carbon layer; (2) 0.5 g of porous carbon layer, 6.7 g of pyrrole, 100 mL of water, and 0.6 g of sodium p-toluenesulfonate were stirred at 60 ° C for 4 h, the product was dried, and then 50 mL of DMF and 11.2 g of erythritol were added, the pH was adjusted to 7.5, and the reaction was stirred at 70 ° C for 2 h. Then 36.4 g of phosphorus trichloride was added, and the reaction was carried out at 40 ° C for 2 h. Then 15.3 g of myristic acid was added, and the reaction was carried out at 45 ° C for 2 h. The product was dried to obtain a porous carbon layer modified product.

[0026] The preparation method of the starch modified material is as follows: add 1.2 g of benzoyl chloride and 15 mL of benzene to 4 g of soluble starch, stir and react at 40 ° C for 40 min, rotary evaporate at 50 ° C, and dry to obtain a starch reactant; then add 20 mL of 70 ° C deionized water to the starch reactant, stir for 40 min, add 0.05 g of ammonium persulfate at 60 ° C to obtain a pregelatinized soluble starch solution; at the same time, add 5.8 g of acrylamide, 2.3 g of hexadecyl dimethyl allyl ammonium chloride and 2 g of N, N-methylenebisacrylamide were mixed and added into 10 mL of deionized water to dissolve, and then the solution was slowly poured into the pre-gelatinized soluble starch solution, and the pH of the soluble starch solution was adjusted to 7.0 with 1 mol / L NaOH aqueous solution. The mixture was reacted for 30 minutes, and the mixed solution became a gel state. Stirring was maintained at 70 ° C for 3 hours, and then the gel was cut into pieces with scissors, placed in an electric blast drying oven at 90 ° C for reaction for 3 hours, and finally taken out and dried for 24 hours, and crushed through an 18-mesh sieve to obtain a starch modification. Embodiment 3

[0027] The preparation method of the flame-retardant, water-washable, moderately compatible water-based acrylic resin coating is prepared according to the following steps: (1) Preparation of core layer emulsion: add 700 g of water, 14 g of emulsifier A (mixed with sodium dodecylbenzene sulfonate and AEO-9 in a mass ratio of 2:1), and 32.5 g of methacrylic acid into a reaction container, mix and stir evenly, heat to 40°C, stir and react for 60 min, add monomer A, 11.8 g of carbonizing agent intermediate, 20 g of DOPO, and 4.2 g of 3,4-epoxy-1-butene, and emulsify for 25 min; heat to 65°C, pass reflux water, heat to 85°C, dropwise add 11 g of ammonium persulfate initiator (dissolved in 30 g of water), dropwise add for 1 h, react for 1.5 h, then add 5.6 g of diethanolamine, adjust the pH to 8, and react at 85°C for 1.5 h to obtain core layer emulsion; (2) All monomers B and 10 g of ammonium persulfate initiator (dissolved in 30 g of water) were added dropwise to the core layer emulsion obtained in step (1) for 1 h, and the mixture was stirred at 80 ° C for 1.5 h. Then, 5 g of porous carbon layer modifier, 4.2 g of DOPO and 1.8 g of 3,4-epoxy-1-butene, 2.1 g of ammonium persulfate initiator (dissolved in 6 g of water) and 1.7 g of starch modifier were added, and the mixture was reacted at 65 ° C for 1 h. The mixture was cooled to 50 ° C, 20 g of AEO-9 emulsifier B was added, and the reaction time was 30 min. Ammonia water was added to adjust the pH value to 7-8 to obtain the flame retardant, washable, and moderately compatible water-based acrylic resin coating. The monomer A is prepared by mixing 47.5 g of ethyl acrylate, 38 g of methyl methacrylate and 45 g of hydroxyethyl acrylate; The monomer B is prepared by mixing 59 g of acrylamide, 38 g of methyl methacrylate, and 73.5 g of hydroxyethyl acrylate.

[0028] The preparation method of the carbon-forming agent intermediate is as follows: Add 6.1g of p-hydroxybenzaldehyde into a beaker, stir and dissolve with 125mL of ethanol, pour into a 250mL three-necked flask, stir at a speed of 250r / min, heat to 55°C, slowly drop 1.65g of ethylenediamine diluted with 10mL of ethanol into the three-necked flask through a constant pressure dropping funnel, add for 30min, continue the reaction for 1.5h, stop heating, cool to room temperature, filter and obtain a light yellow crude carbon-forming intermediate, wash with ethanol three times, and vacuum dry at 60°C for 21h to obtain a light yellow carbon-forming intermediate powder, which is a carbon-forming agent intermediate.

[0029] The preparation method of the porous carbon layer modified material is as follows: (1) Cut the vegetable tanned leather scraps into blocks with a length and width of 1 cm, place them in a vacuum tube furnace, heat them at 400°C for 3.5 h for pre-carbonization under a nitrogen atmosphere, mix the obtained carbonized product with KOH in a mass ratio of 1:3, then add 300% water by weight to the above mixture, and stir it at 40-50°C for 20 h, then dry the product, and carbonize it again at 550°C for 1.5 h under nitrogen protection, and finally dry it to obtain a porous carbon layer; (2) 0.5 g of porous carbon layer, 5.6 g of pyrrole, 100 mL of water, and 0.5 g of sodium p-toluenesulfonate were stirred at 55 °C for 3 h. The product was dried. Then, 50 mL of DMF and 9.68 g of erythritol were added, the pH was adjusted to 7.5, and the mixture was stirred and reacted at 60 °C for 1.5 h. Then, 31.9 g of phosphorus trichloride was added, and the mixture was reacted at 35 °C for 1.5 h. Then, 13.9 g of myristic acid was added, and the mixture was reacted at 40 °C for 1.5 h. The product was dried to obtain a porous carbon layer modified product.

[0030] The preparation method of the starch modified material is as follows: 1.1 g of benzoyl chloride and 15 mL of benzene are added to 4 g of soluble starch, the mixture is stirred at 35 ° C for 35 min, and the mixture is rotary evaporated at 45 ° C and dried to obtain a starch reactant; 20 mL of 70 ° C deionized water is added to the starch reactant, the mixture is stirred for 35 min, and 0.04 g of ammonium persulfate is added at 55 ° C to obtain a pregelatinized soluble starch solution; 5.8 g of acrylamide, 2.3 g of hexadecyl dimethyl allyl ammonium chloride and 2 g of N, N-methylene bisacrylamide are mixed, added to 10 mL of deionized water to dissolve, and then the solution is slowly poured into the pregelatinized soluble starch solution, the pH of the soluble starch solution is adjusted to 7.0 with a 1 mol / L NaOH aqueous solution, and the mixture is reacted for 22.5 min, the mixed solution becomes a gel state, and the mixture is stirred at 65 ° C for 2.5 h, and then the gel is cut into pieces with scissors, placed in an electric hot air drying oven at 90 ° C for reaction for 2.5 h, and finally taken out and dried for 24 h, crush through an 18-mesh sieve to obtain a starch modification; The prepared acrylic resin coating was poured into a polytetrafluoroethylene mold with a thickness of 3 mm, and a droplet test, cone calorimetry and other tests were performed.

[0031] Droplet test (1) Sample preparation: Place the prepared acrylic resin film in a constant temperature and humidity chamber set at 23°C ± 0.5°C and 50% ± 5% humidity for 48 h. Then take it out and cut it into samples of 110 cm × 10 cm × 3 mm. Prepare 2 sets of samples, with 5 samples in each set.

[0032] (2) Parameters: Clamp about 5mm from the top so that the sample is vertically downward. Place a rosin board at the bottom of the sample, and pad about 0.3g of absorbent cotton on the board, evenly placed on the board. Adjust the gas flow rate to 105±5 mL / min so that the flame height reaches 20±1mm. Set the combustion time to 10s.

[0033] (3) Flame recording: After setting the parameters, start the flame ignition. After the 10s ignition, press the afterflame time start button. When the sample combustion is finished and only sparks are left, press the afterflame combustion end button and enter the afterburning time. When the flame is completely extinguished, press the afterburning time end button and record the burning afterflame time and afterburning time.

[0034] (4) Molten droplet observation: During the combustion process, pay attention to whether the combustion produces molten droplets, and whether the molten droplets dripping onto the cotton wool below will cause secondary combustion. Record the observation results.

[0035] The ASTM E1354-1990 (2004 standard) was used, and the cone calorimeter 2000 of the British FTT company was used for analysis and determination. The sample was 10cm×10cm, the thickness was 3mm, and the thermal radiation power was 12kW / m 2 , determine the maximum heat release rate pkHHR kW / m 2 ,THR total heat release MJ / m².

[0036] Take 28 parts of acrylic resin coatings from Examples 1 to 3, 0.2 parts of carboxymethyl fiber, 4 parts of polyvinyl pyrrolidone PVP-K30, 3 parts of polyvinyl alcohol, 6 parts of polyethylene glycol, and 1.5 parts of polyoxyethylene polypropylene ether, respectively, add them to 35 parts of distilled water in sequence, stir evenly, add 2.5 parts of polypropylene glycol (PPG-400), 0.5 parts of leveling agent, 0.6 parts of silane coupling agent, stir evenly, filter and let stand to defoam, and record it as the application plan.

[0037] The coating solutions of Examples 1 to 3 were sprayed on the epoxy resin circuit board respectively, dried at 70°C for 30 min, and washed with a 50°C warm water solution (temperature controlled at 50°C, KMnO4 50g / L, potassium manganate 10g / L, amplitude controlled at 20mm / s, sodium hydroxide 1mol / L, and the rest was water); The water washing test method: Determination of the film removal time of the reference compound liquid coating [1] Xie Dan, Jia Danfeng. About water-washable temporary protective coatings [J]. Aging and Application of Synthetic Materials, 2017, 46(5): 43~50.

[0038] The PCB hole position accuracy is measured by sampling and slicing under a metallographic microscope, and the hole wall roughness is measured by a secondary element device; the hole position accuracy, hole wall roughness, and hole diameter melt are sprayed with an application solution (coating thickness 0.04mm) on the aluminum foil (0.1mm), and the lower PCB board is drilled.

[0039] The drill bit temperature is measured using a hot red temperature detector; The pore size melt is observed by naked eyes, and the results are compared and divided into small, less and more data (if less than 30 holes have melt out of 100 holes, it is defined as small, 31 to 70 holes are less, and 71 to 100 holes are more); The adhesion of the compound liquid coating is determined according to GB / T 9286-1998 and ISO 2409:1992. The soft substrate is an epoxy resin board. A blade is used to scratch 100 small squares of 1mm × 1mm on the coating sample, and then they are bonded with transparent tape. The degree of damage to the paint film is observed to determine the adhesion level of the paint film. The results are expressed in levels of 0 to 5, with 0 being the worst and 5 being the best. The compatibility is moderate at level 2.

[0040] Table 1 Properties of flame retardant, water-washable, moderately compatible water-based acrylic resin coatings: index Embodiment 1 Embodiment 2 Embodiment 3 Comparative Example HkDJ 208.3 205.8 201.6 336.7 THR 33.4 31.6 32.8 92.5 Droplet situation No dripping No dripping No dripping No dripping Water washability (50℃,s) 39 36 38 211 Hole position accuracy (mil) 1.6 1.8 1.5 2.6 Hole wall roughness (μm) 7 8 6 24 Drill bit temperature (℃) 75 82 89 102 Pore ​​size melt few few few many Adhesion (grade) 2 2 2 3 The second embodiment of 202011318656.X is used as a comparative example, and the same amount is substituted under the same conditions. The flame retardancy, water washability and compatibility of the present invention are improved compared with the comparative example. The PCB board aperture melt of the present invention example is less and easy to clean, and the film around the aluminum cover plate is almost not bonded after the drill bit is heated. However, in the comparative document, the film around the aluminum cover plate is bonded after the drill bit is heated, and the PCB board aperture melt is more and difficult to clean.

[0041] The following study was conducted by performing a comparative experiment using Example 2.

[0042] Table 2 Flame retardant, water washable, moderately compatible water-based acrylic resin coating properties: index Embodiment 2 No added material HkDJ 316.3 Unadded carbon agent intermediate THR 38.6 Unadded carbon agent intermediate Droplet situation A small amount of molten droplets Unadded carbon agent intermediate Hole position accuracy (mil) 3.6 Unadded carbon agent intermediate Hole wall roughness (μm) 19 Unadded carbon agent intermediate Drill bit temperature (℃) 85 Unadded carbon agent intermediate Pore ​​size melt many Unadded carbon agent intermediate As shown in Table 2, the carbonizing agent intermediate not only affects the flame retardancy of the acrylic resin film (pkHHR, THR and molten droplet), but also affects the drilling accuracy and aperture roughness (acrylic resin film sprayed on the aluminum cover plate, the drilling accuracy and aperture roughness of the PCB and the aperture melt) and the drill temperature. As shown in Table 2, the indicators without the addition of the carbonizing agent intermediate are not as good as those with the addition of the above substances.

[0043] Table 3 Effects of porous carbon layer modifiers on flame retardant, water-washable, moderately compatible water-based acrylic resins and their application properties: index Example 2 No added material HkDJ 298.4 Without porous carbon layer modification THR 39.6 Without porous carbon layer modification Droplet situation There are a lot of molten drops falling Without porous carbon layer modification Hole position accuracy (mil) 4.5 Without porous carbon layer modification Hole wall roughness (μm) 28 Without porous carbon layer modification Drill bit temperature (℃) 103 Without porous carbon layer modification Pore ​​size melt many Without porous carbon layer modification HkDJ 264.6 Porous carbon layer modifier added, but no erythritol added THR 35.4 Porous carbon layer modifier added, but no erythritol added Melt drop situation A small amount of molten droplets Porous carbon layer modifier added, but no erythritol added Drill bit temperature (℃) 89 Porous carbon layer modifier added, but no erythritol added Aperture Melt less Porous carbon layer modifier added, but no erythritol added HkDJ 276.2 Porous carbon layer modifier, but no myristic acid THR 36.1 Porous carbon layer modifier, but no myristic acid Melt drop situation A small amount of molten droplets Porous carbon layer modifier, but no myristic acid Drill bit temperature (℃) 86 Porous carbon layer modifier, but no myristic acid Aperture Melt less Porous carbon layer modifier, but no myristic acid Hole position accuracy (mil) 2.8 Porous carbon layer modifier, but no myristic acid Hole wall roughness (μm) 16 Porous carbon layer modifier, but no myristic acid Drill bit temperature (℃) 91 Add porous carbon layer modifier, but not phosphorus trichloride Aperture Melt less Add porous carbon layer modifier, but not phosphorus trichloride As shown in Table 3, the porous carbon layer modifier, phosphorus trichloride, myristic acid and erythritol can improve the flame retardancy, pore position accuracy and pore wall roughness of acrylic resin.

[0044] Table 4 Effects of starch modifications on flame retardant, water-washable, moderately compatible water-based acrylic resins and their application properties: index Example 2 No added material Melt drop situation A small amount of molten droplets No starch modification Drill bit temperature (℃) 88 No starch modification Aperture Melt less No starch modification Hole position accuracy (mil) 3.7 No starch modification Hole wall roughness (μm) 18 No starch modification Water washability (50℃,s) 90 No starch modification Droplet situation A small amount of molten droplets Add starch modification, no benzoyl chloride Drill bit temperature (℃) 82 Add starch modification, no benzoyl chloride Pore ​​size melt few Add starch modification, no benzoyl chloride Hole position accuracy (mil) 2.6 Add starch modification, no benzoyl chloride Hole wall roughness (μm) 13 Add starch modification, no benzoyl chloride Water washability (50℃,s) 52 Add starch modification, no benzoyl chloride Water washability (50℃,s) 57 With starch modification, without N,N-methylenebisacrylamide Water washability (50℃,s) 68 Add starch modification, without adding hexadecyl dimethyl allyl ammonium chloride It can be found from Table 4 that the adhesion of the acrylic resin obtained without adding the above substances is not level 2, the time used for water washability is increased, and the hole position accuracy and hole wall roughness are reduced, indicating that starch modification, benzoyl chloride, N,N-methylenebisacrylamide and hexadecyldimethylallyl ammonium chloride play a significant role in improving the water washability and compatibility of acrylic resin coatings.

[0045] In addition, the pkHHR and THR of the acrylic resin film without the addition of 3,4-epoxy-1-butene and diethanolamine increased, and the water washability of the film was reduced without the addition of acrylamide and hydroxyethyl acrylate.

Claims

1. A method for preparing a flame-retardant, water-washable, moderately compatible water-based acrylic resin coating, characterized in that: Prepare according to the following steps: (1) Preparation of core layer emulsion: add 600-800 g of water, 11-17 g of emulsifier A, and 24-41 g of methacrylic acid to a reaction container, mix and stir evenly, heat to 40-45°C, stir and react for 60 min, then add monomer A, 10.2-13.4 g of carbonizing agent intermediate, 18.3-21.6 g of DOPO, and 2.1-6.3 g of 3,4-epoxy-1-butene, and emulsify for 20-30 min; heat to 65°C, pass reflux water, heat to 80-90°C, dropwise add 10-12 g of initiator, dropwise add for 1-1.5 h, react for 1-2 h, then add 3.15-8.4 g of diethanolamine, adjust the pH to 8, and react at 80-90°C for 1-2 h to obtain core layer emulsion; (2) To the whole core layer emulsion obtained in step (1), all monomers B and 8-12g of initiator are added dropwise at the same time for 1h, and the mixture is stirred at 75-85°C for 1.5h. Then, 4.6-5.5g of porous carbon layer modifier, 4.1-4.3g of DOPO, 1.2-2.4g of 3,4-epoxy-1-butene, 2.1g of initiator and 1.1-2.3g of starch modifier are added, and the mixture is reacted at 60-70°C for 1h. The mixture is cooled to 50°C, 14-20g of emulsifier B is added, and the reaction time is 30min. Ammonia water is added to adjust the pH value to 7-8 to obtain a flame-retardant, washable, and moderately compatible water-based acrylic resin coating. The monomer A is prepared by mixing 40-55g of ethyl acrylate, 28-48g of methyl methacrylate and 38-52g of hydroxyethyl acrylate; The monomer B is prepared by mixing 49-69 g of acrylamide, 12-54 g of methyl methacrylate and 55-92 g of hydroxyethyl acrylate.

2. The method for preparing a flame-retardant, washable, moderately compatible water-based acrylic resin coating according to claim 1, characterized in that: The emulsifier A is prepared by mixing sodium dodecylbenzene sulfonate and AEO-9 in a mass ratio of 2:

1.

3. The method for preparing a flame-retardant, washable, moderately compatible water-based acrylic resin coating according to claim 1, characterized in that: The preparation method of the carbon-forming agent intermediate is as follows: Add 6.1g of p-hydroxybenzaldehyde into a beaker, stir and dissolve with 100-150mL of ethanol, pour into a 250mL three-necked flask, stir at a speed of 250r / min, heat to 50-60°C, slowly drop 1.5-1.8g of ethylenediamine diluted with 10mL of ethanol into the three-necked flask through a constant pressure dropping funnel for 30min, continue the reaction for 1-2.5h, stop heating, cool to room temperature, filter and obtain a light yellow crude carbon-forming intermediate, wash with ethanol three times, and vacuum dry at 60°C for 18-24h to obtain a light yellow carbon-forming intermediate powder, which is a carbon-forming agent intermediate.

4. The method for preparing a flame-retardant, washable, moderately compatible water-based acrylic resin coating according to claim 1, characterized in that: The initiator is any one of ammonium persulfate and potassium persulfate.

5. The method for preparing a flame-retardant, washable, moderately compatible water-based acrylic resin coating according to claim 1, characterized in that: The preparation method of the porous carbon layer modified material is as follows: (1) Cut the vegetable tanned leather scraps into blocks with a length and width of 1 cm, place them in a vacuum tube furnace, heat them at 400°C for 3-4 h in a nitrogen atmosphere for pre-carbonization, mix the obtained carbonized product with KOH in a weight ratio of 1:3, then add 300% water by weight to the mixture, and stir at 40-50°C for 18-22 h, then dry the product, and then carbonize and keep it warm at 500-600°C for 1-2 h under nitrogen protection, and finally dry it to obtain a porous carbon layer; (2) 0.5 g of porous carbon layer, 4.5-6.7 g of pyrrole, 100 mL of water, and 0.4-0.6 g of sodium p-toluenesulfonate were stirred at 50-60 °C for 2-4 h, and the product was dried. Then, 50 mL of DMF and 8.17-11.2 g of erythritol were added, and the pH was adjusted to 7.

5. The mixture was stirred and reacted at 50-70 °C for 1-2 h. Then, 27.4-36.4 g of phosphorus trichloride was added, and the mixture was reacted at 30-40 °C for 1-2 h. Then, 12.5-15.3 g of myristic acid was added, and the mixture was reacted at 30-45 °C for 1-2 h. The product was dried to obtain a porous carbon layer modified product.

6. The method for preparing a flame-retardant, washable, moderately compatible water-based acrylic resin coating according to claim 1, characterized in that: The preparation method of the starch modified material is as follows: add 1-1.2 g of benzoyl chloride and 15 mL of benzene to 4 g of soluble starch, stir and react at 30-40 ° C for 30-40 min, rotary evaporate at 40-50 ° C, and dry to obtain a starch reactant; then add 20 mL of 70 ° C deionized water to the starch reactant, stir for 30-40 min, add 0.03-0.05 g of ammonium persulfate at 50-60 ° C to obtain a pregelatinized soluble starch solution; then mix 5.8 g of acrylamide, 2.3 g of hexadecyl dimethyl allyl ammonium chloride and 2 g of N, N-methylene bisacrylamide, add to 10 mL of deionized water to dissolve, then slowly pour the solution into the pregelatinized soluble starch solution, and use 1 mol / L NaOH Adjust the solution pH to 7.0, react for 15-30 minutes, the mixed solution becomes a gel state, stir at 60-70°C for 2-3 hours, then cut the gel into pieces with scissors, place it in an electric heated blast drying oven at 90°C for 2-3 hours, finally take it out and dry it for 24 hours, crush it through an 18-mesh sieve to obtain the starch modification.

7. The method for preparing a flame-retardant, washable, moderately compatible water-based acrylic resin coating according to claim 1, characterized in that: The emulsifier B is AEO-9.

Citation Information

Patent Citations

  • Manufacturing method for improving accuracy of PCB (printed circuit board) back drilling hole

    CN103533761A

  • Anti-carburizing painting capable of being removed through washing after quenching and preparation method thereof

    CN105132651A

  • Gluing aluminum-based cover plate for PCB drilling and preparing method thereof

    CN110281308A

  • Preparation method of flame-retardant core-shell type environment-friendly water-based resin coating

    CN112322132A

  • Washable temporary decorative coating for soft PVC (polyvinyl chloride) as well as preparation method and application of washable temporary decorative coating

    CN114921135A