Waterborne acrylate modified polyurethane dispersion as well as preparation method and application thereof

By using a hydrophobic blocking agent to modify the polyurethane prepolymer in aqueous two-component silver powder paint, an aqueous acrylate modified polyurethane dispersion with core-shell structure is solved, and the sag and orientation of silver powder paint in high humidity environments is solved. Poor problems, achieving excellent water resistance and flash effect.

CN118931302AActive Publication Date: 2024-11-12GUANGZHOU KINTE IND +1

Patent Information

Application Number
CN202411152185.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing water-based two-component silver powder paint has problems of poor direction of sag and silver powder during construction, which makes it unable to meet the water resistance and metallicity requirements of high-end fields under high humidity and high film thickness environments.

Method used

Modify the polyurethane prepolymer by hydrophobic blocking agents (such as linoleic acid and n-octadecanol) to synthesize modified polyurethane with hydrophobic terminals and carbon-carbon double bond structures to form a core-shell structure to modify the aqueous acrylic acid ester The polyurethane dispersion improves thickening and thixotropic properties through hydrogen bonding and transient mesh structure, ensuring the orientation arrangement and flashing effect of silver powder.

Benefits of technology

It significantly improves the water resistance, silver powder orientation and flash effect of water-based two-component silver powder paint, solves the problems of sag and poor orientation, and meets the application requirements in high-end fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003946530000181
    Figure BDA0005003946530000181
  • Figure BDA0005003946530000201
    Figure BDA0005003946530000201
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and particularly relates to a waterborne acrylate modified polyurethane dispersion as well as a preparation method and application thereof. The water-based acrylate modified polyurethane dispersion disclosed by the invention has a core-shell structure; the core of the core-shell structure comprises modified polyurethane; a shell layer of the core-shell structure comprises polyacrylate; the modified polyurethane is obtained by modifying a polyurethane prepolymer with an end-capping reagent 1; the end-capping reagent 1 comprises at least one of linoleic acid and n-octadecanol. Hydrophobic modified polyurethane serves as a core, polyacrylate is grafted to the core through free radical polymerization reaction, and the waterborne acrylate modified polyurethane dispersoid of a core-shell structure is obtained. The modified polyurethane is connected with a hydrophilic chain segment of a shell layer through a hydrogen bond through a polyurethane core, a transient grid structure is formed, a thickening phenomenon and thixotropic performance are generated, the directional arrangement and flashing effect of silver powder in the silver powder paint is improved, and the water resistance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and particularly relates to a waterborne acrylate modified polyurethane dispersion and a preparation method and application thereof. Background Art

[0002] Traditional solvent-based coatings do not meet current environmental protection requirements because they contain a large amount of volatile organic compounds (VOCs). Water-based coatings use water as a dispersion medium to replace organic solvents in whole or in large part, which greatly reduces the use and emission of volatile organic compounds, reduces the harm and pollution to the environment during the production and construction of coatings, and becomes one of the main development directions of green and environmentally friendly coatings. Water-based acrylate-modified polyurethane dispersion (PUA) is called the "third generation of water-based polyurethane", in which polyacrylate (PA) has excellent solvent resistance, mechanical properties, water resistance, weather resistance and light and color retention, while polyurethane (PU) has excellent wear resistance, cold resistance and flexibility. However, due to the large amount of hydrophilic monomers introduced into the molecular chain segment during the water-based process of polyurethane, its water resistance is reduced and the thickening effect is poor, which greatly limits the application scope of water-based polyurethane coatings.

[0003] Water-based two-component silver paint is favored by people for its rich colors, excellent angle-dependent color effects and elegant metal decorative effects, and is widely used in heating equipment, metal pipes, auto parts, plastic panels and other fields. At present, the coating of silver paint on metal surfaces in China mainly adopts a composite coating process of single-component silver paint and clear varnish. The coating process is complicated and the coating cost is high, which is not conducive to large-scale promotion and application. The use of two-component water-based acrylic modified polyurethane silver powder paint to replace the single-component silver powder paint and topcoat varnish composite coating process can simplify the existing construction process to a certain extent, which is beneficial to reduce the coating costs of downstream customers. However, due to the large latent heat of water in the system and the slow volatilization rate, the water-based acrylic modified polyurethane silver powder paint is prone to cause water-based two-component silver powder paint to have shortcomings such as sagging, silver powder sedimentation, and poor directional arrangement of silver powder. The flaky aluminum powder cannot be "lying flat" in the wet film or dry film during the spraying or film-forming process, resulting in the silver powder paint being blackened, flowery, and the gloss, vividness and metallic feel cannot meet the requirements. In the coating formula of conventional water-based two-component silver powder paint, rheological additives such as low-shear viscosity thickeners, non-Newtonian pseudoplastic thickeners, and organic bentonite thixotropic agents are often used to adjust the viscosity and thixotropy of the water-based silver powder paint system, thereby enhancing the silver powder's orientation, anti-sagging, and anti-settling effects. However, when the resin system contains a large amount of hydrophilic solvents or hydrophilic groups, the thickening efficiency of water-based rheological additives is extremely low, resulting in the water-based silver powder paint being unable to be used in high-end fields with high humidity, high film thickness, and strong metallic feel requirements.

[0004] Therefore, there is an urgent need to provide a water-based acrylate-modified polyurethane dispersion, which has good thickening, thixotropy, and water resistance, and the prepared silver powder paint has excellent silver powder directional arrangement effect and sparkling effect. Summary of the invention

[0005] The present invention aims to solve one or more technical problems existing in the above-mentioned prior art, and at least provide a beneficial choice or create conditions. Specifically, the present invention provides a water-based acrylate modified polyurethane dispersion, which has good thickening, thixotropy and water resistance, and the prepared silver powder paint has excellent water resistance, silver powder directional arrangement effect and glitter effect.

[0006] The inventive concept of the present invention is as follows: the water-based acrylate-modified polyurethane dispersion of the present invention has a core-shell structure; the core of the core-shell structure includes modified polyurethane; the shell layer of the core-shell structure includes polyacrylate; the modified polyurethane is obtained by modifying a polyurethane prepolymer with a capping agent 1; the capping agent 1 includes at least one of linoleic acid and n-octadecyl alcohol. The invention adopts a hydrophobic end-capping agent to modify a polyurethane prepolymer to synthesize a polyurethane with a hydrophobic end and a carbon-carbon double bond structure. In an aqueous acrylate modified polyurethane dispersion, since the modified polyurethane has the hydrophobic end structure, the aqueous acrylate modified polyurethane dispersion can have a strong association and hydrogen bonding effect in an emulsion and a resin. In the aqueous acrylate modified polyurethane dispersion with a core-shell structure, the hydrophobic ends of the polyurethane core are mutually associated to form micelles, and the modified polyurethane with the hydrophobic end can be connected through the hydrophilic chain segments of the polyacrylate shell layer through the polyurethane core through hydrogen bonds to form a transient grid structure, thereby generating a thickening phenomenon and thixotropic performance, and improving water resistance, so that the prepared silver powder paint has excellent water resistance, silver powder directional arrangement effect and flashing effect.

[0007] Therefore, a first aspect of the present invention provides an aqueous acrylate-modified polyurethane dispersion.

[0008] Specifically, the aqueous acrylate modified polyurethane dispersion has a core-shell structure; the core of the core-shell structure includes modified polyurethane; the shell layer of the core-shell structure includes polyacrylate;

[0009] The modified polyurethane is obtained by modifying the polyurethane prepolymer with the end-capping agent 1;

[0010] The end-capping agent 1 includes at least one of linoleic acid and n-octadecyl alcohol.

[0011] Specifically, the end-capping agent 1 is used as a long carbon chain end-capping agent, mainly for hydrophobic modification of polyurethane prepolymer. The waterborne acrylate modified polyurethane dispersion of the present invention is a self-emulsifying and surfactant-free environmentally friendly waterborne resin, which has thixotropy and helps the directional arrangement of silver powder.

[0012] Preferably, the preparation method of the modified polyurethane comprises the following steps:

[0013] (1) vacuum dehydrating the polymer polyol, adding catalyst 1 and isocyanate monomer, and carrying out reaction 1 to obtain polyurethane prepolymer I; adding catalyst 2 and chain extender to the polyurethane prepolymer I, and carrying out reaction 2 to obtain polyurethane prepolymer II;

[0014] (2) The end-capping agent 1, the end-capping agent 2 and the polyurethane prepolymer II obtained in step (1) are mixed and reacted with each other to obtain the modified polyurethane.

[0015] Preferably, in step (1), the polymer polyol includes at least one of polyether polyol and polyester polyol.

[0016] Preferably, in step (1), the catalysts 1 and 2 both comprise dibutyltin dilaurate.

[0017] Preferably, in step (1), the isocyanate monomer includes at least one of isophorone diisocyanate and 4,4'-dicyclohexylmethane diisocyanate.

[0018] Preferably, in step (1), the chain extender includes at least one of diethylene glycol, dimethylol propionic acid, and 1,4-butanediol-2-sodium sulfonate.

[0019] Preferably, in step (1), the vacuum degree of the vacuum dehydration is 0.08-0.095 MPa, the temperature of the vacuum dehydration is 50-70°C, and the time of the vacuum dehydration is 0.8-1.2 h; further preferably, in step (1), the vacuum degree of the vacuum dehydration is 0.085-0.095 MPa, the temperature of the vacuum dehydration is 55-65°C, and the time of the vacuum dehydration is 0.9-1.1 h; further preferably, in step (1), the vacuum degree of the vacuum dehydration is 0.09 MPa, the temperature of the vacuum dehydration is 60°C, and the time of the vacuum dehydration is 1 h.

[0020] Preferably, in step (1), the reaction temperature of reaction 1 is 75-90°C, and the reaction time of reaction 1 is 1.5-2.5h; further preferably, in step (1), the reaction temperature of reaction 1 is 80-90°C, and the reaction time of reaction 1 is 1.8-2.2; further preferably, in step (1), the reaction temperature of reaction 1 is 85°C, and the reaction time of reaction 1 is 2h.

[0021] Preferably, in step (1), the reaction temperature of reaction 2 is 55-75°C, and the reaction time of reaction 2 is 2.5-3.5h; further preferably, in step (1), the reaction temperature of reaction 2 is 60-70°C, and the reaction time of reaction 2 is 2.7-3.3h; further preferably, in step (1), the reaction temperature of reaction 2 is 65°C, and the reaction time of reaction 2 is 3h.

[0022] Specifically, step (1) obtains a polyurethane prepolymer having an isocyanate (-NCO) terminal group.

[0023] Preferably, in step (2), the end-capping agent 1 comprises at least one of linoleic acid and n-octadecyl alcohol.

[0024] Preferably, in step (2), the end-capping agent 2 comprises 2-hydroxyethyl methacrylate.

[0025] Preferably, in step (2), the reaction temperature of reaction 3 is 65-85°C, and the reaction time of reaction 3 is 2.0-3.0h; further preferably, in step (2), the reaction temperature of reaction 3 is 70-80°C, and the reaction time of reaction 3 is 2.2-2.8h; further preferably, in step (2), the reaction temperature of reaction 3 is 75°C, and the reaction time of reaction 3 is 2.5h.

[0026] Specifically, linoleic acid (LA) and n-octadecyl alcohol are used as end-capping agents for long carbon chains, mainly for hydrophobic modification; 2-hydroxyethyl methacrylate (HEMA) is used as an end-capping agent to complete the -NCO end-capping, and because it contains a carbon-carbon double bond, it can form a conjugated double bond with the 8th, 9th, 10th, and 11th carbon atoms of linoleic acid (LA), and at the same time provide an active reaction site for the subsequent free radical copolymerization reaction.

[0027] Preferably, in the modified polyurethane, the molar ratio of the isocyanate group (-NCO) to the hydroxyl group (-OH) is 1.0-1.5:1; further preferably, in the modified polyurethane, the molar ratio of the -NCO to -OH is 1.05-1.45:1.

[0028] The second aspect of the present invention provides a method for preparing the waterborne acrylate-modified polyurethane dispersion described in the first aspect of the present invention.

[0029] Specifically, the preparation method of the waterborne acrylate modified polyurethane dispersion comprises the following steps:

[0030] (1) mixing an acrylate monomer and an initiator to obtain a mixture, taking a portion of the mixture and mixing it with a modified polyurethane and a neutralizer, and emulsifying to obtain a mixed emulsion;

[0031] (2) mixing the remaining mixture with the mixed emulsion obtained in step (1), reacting the mixture, and obtaining the water-based acrylate-modified polyurethane dispersion.

[0032] Specifically, step (1) adopts a pre-monomer emulsification process, and the role of adding part of the acrylic ester monomer and part of the initiator is to reduce the viscosity of the modified polyurethane, improve the success rate of phase inversion emulsification, and act as both a solvent and a raw material for acrylic acid modification, avoiding the use of emulsifiers and improving the water resistance of the resin after film formation. The present invention uses hydrophobic modified polyurethane as the core, and grafts polyacrylate on the core through free radical polymerization to obtain a water-based acrylate modified polyurethane dispersion with a core-shell structure.

[0033] Specifically, step (1) is carried out at room temperature, so step (1) is only a physical mixing of the raw material components, and no chemical reaction occurs.

[0034] Preferably, the mass ratio of the acrylate monomer to the modified polyurethane is 4:(4-6); further preferably, the mass ratio of the acrylate monomer to the modified polyurethane is 4:(4.5-5.5); further preferably, the mass ratio of the acrylate monomer to the modified polyurethane is 4:5.

[0035] Preferably, the emulsification method is to add deionized water in a high-speed dispersion state to complete the emulsification treatment of the modified polyurethane.

[0036] Preferably, in step (2), the reaction temperature is 65-85°C, and the reaction time is 1.5-2.5h; further preferably, in step (2), the reaction temperature is 70-80°C, and the reaction time is 1.8-2.2h; further preferably, in step (2), the reaction temperature is 75°C, and the reaction time is 2h.

[0037] Preferably, the remaining mixture is added dropwise into the mixed emulsion obtained in step (1) for mixing.

[0038] Preferably, the post-initiation reaction is carried out after the reaction is complete.

[0039] Specifically, the post-initiation reaction refers to extending the reaction time or adding additional initiators (generally 0.1% of the total amount of reaction initiators) to consume the remaining trace monomers in the reaction system or further increase the molecular weight.

[0040] Preferably, the time of the post-initiation reaction is 0.8-1.2 h, more preferably, the time of the post-initiation reaction is 0.9-1.1 h, and even more preferably, the time of the post-initiation reaction is 1 h.

[0041] Preferably, the acrylic ester monomer includes at least one of methacrylic acid, isobornyl methacrylate, isobutyl methacrylate, glycidyl methacrylate, isooctyl methacrylate, methyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, acrylic acid, n-butyl acrylate, acrylamide, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, cyclohexyl acrylate, styrene, and isobornyl acrylate.

[0042] Preferably, the initiator includes at least one of tert-butyl perbenzoate, di-tert-butyl peroxide, azobisisobutyronitrile, di-tert-amyl peroxide, potassium persulfate, ammonium persulfate and sodium persulfate.

[0043] Preferably, the neutralizing agent comprises an amine neutralizing agent; further preferably, the neutralizing agent comprises triethylamine.

[0044] A third aspect of the present invention provides a silver powder paint.

[0045] Specifically, the silver powder paint includes the water-based acrylate-modified polyurethane dispersion described in the first aspect of the present invention.

[0046] Preferably, the silver powder paint comprises component A and component B; the component A comprises waterborne acrylate modified polyurethane dispersion, cosolvent A, and silver powder; and the component B comprises isocyanate curing agent and cosolvent B.

[0047] More preferably, the A component also includes water, an auxiliary agent

[0048] Preferably, the mass ratio of component A to component B is 4.5-8.5:1; further preferably, the mass ratio of component A to component B is 5-8:1.

[0049] Specifically, component A and component B are stored separately, and when needed, component A and component B can be mixed according to the above mass ratio.

[0050] Preferably, the isocyanate curing agent comprises a hydrophilic aliphatic polyisocyanate; further preferably, the isocyanate curing agent comprises hexamethylene diisocyanate (HDI).

[0051] Preferably, the co-solvent A and the co-solvent B independently include at least one of ethylene glycol butyl ether, propylene glycol butyl ether, dipropylene glycol butyl ether, dipropylene glycol methyl ether, and propylene glycol methyl ether acetate.

[0052] Preferably, the auxiliary agent is an aqueous auxiliary agent.

[0053] Preferably, the additive includes at least one of a neutralizer, a wetting agent, a dispersant, a leveling agent, a rheological additive, a thixotropic additive, a silver powder orientation additive, an anti-flash rust agent, and a defoaming agent.

[0054] Preferably, the neutralizing agent comprises an organic alcohol amine neutralizing agent.

[0055] Preferably, the wetting agent comprises a fluorine-silicon hybrid wetting agent.

[0056] Preferably, the dispersant comprises a polyurethane modified acrylic copolymer dispersant.

[0057] Preferably, the leveling agent comprises a fluorine-modified acrylate leveling agent.

[0058] Preferably, the rheological additive comprises a nonionic polyurethane low shear thickener.

[0059] Preferably, the thixotropic agent comprises an inorganic colloidal mineral thixotropic agent.

[0060] Preferably, the silver powder orientation aid comprises a polyamide wax type silver powder orientation aid.

[0061] Preferably, the flash rust inhibitor comprises a phosphate and a mixture of multiple organic composite acids.

[0062] Preferably, the defoaming agent comprises a block copolymer defoaming agent of polyoxyethylene and polyoxypropylene.

[0063] Preferably, by weight, the component A comprises 45-65 parts of waterborne acrylate modified polyurethane dispersion, 4.5-11 parts of cosolvent A, 4.5-11 parts of silver powder, 0.9-8 parts of auxiliary agent, and 18-35 parts of water; the component B comprises 11-18 parts of isocyanate curing agent and 3.5-6.5 parts of cosolvent B.

[0064] Further preferably, in parts by weight, the component A comprises 50-60 parts of water-based acrylate modified polyurethane dispersion, 5-10 parts of cosolvent A, 5-10 parts of silver powder, 1-5 parts of auxiliary agent, and 20-32 parts of water; the component B comprises 12-17 parts of isocyanate curing agent and 4-6 parts of cosolvent B.

[0065] Specifically, the molecular structure of the waterborne acrylate modified polyurethane dispersion of the present invention includes a modified polyurethane core with a hydrophobic end and a hydroxyl-containing polyacrylic acid shell, so that it can undergo a cross-linking reaction with an isocyanate curing agent to prepare a two-component waterborne coating. At the same time, the unique self-thickening and thixotropic properties of the hydrophobically modified polyurethane core are conducive to improving the directional arrangement and flash effect of silver powder in the waterborne two-component silver powder paint, and can better solve the problems of sagging and poor silver powder orientation in the construction process of the existing waterborne two-component silver powder paint.

[0066] Preferably, the method for preparing the silver powder paint comprises the following steps:

[0067] (1) mixing the raw material components of component A to obtain component A;

[0068] (2) The raw material components of component B are mixed to obtain component B; the component A and the component B constitute the silver powder paint.

[0069] Preferably, in step (1), the silver powder is first prepared into a silver powder paste, and then mixed with other components to obtain the component A.

[0070] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0071] (1) The aqueous acrylate modified polyurethane dispersion of the present invention is a self-emulsifying and surfactant-free environmentally friendly aqueous resin, which has thixotropy and is conducive to the directional arrangement of silver powder. The present invention uses a hydrophobic end-capping agent (octadecyl alcohol and / or linoleic acid) to modify a polyurethane prepolymer to synthesize a modified polyurethane having a hydrophobic end and a carbon-carbon double bond structure. In the aqueous acrylate modified polyurethane dispersion, since the modified polyurethane has a hydrophobic end structure, the aqueous acrylate modified polyurethane dispersion can have a strong association and hydrogen bonding effect in the emulsion and the resin. The hydrophobic ends of the polyurethane core in the aqueous acrylate modified polyurethane dispersion with a core-shell structure associate with each other to form micelles, and the modified polyurethane with a hydrophobic end can be connected by hydrogen bonding through the polyurethane core and the hydrophilic chain segment of the polyacrylate shell layer to further form a transient grid structure, thereby generating a thickening phenomenon and thixotropic properties, and can improve water resistance and mechanical properties.

[0072] (2) The molecular structure of the waterborne acrylate modified polyurethane dispersion of the present invention includes a modified polyurethane core with a hydrophobic end and a hydroxyl-containing polyacrylic acid shell, so that it can undergo a cross-linking reaction with an isocyanate curing agent to prepare a two-component waterborne coating. At the same time, the unique self-thickening and thixotropic properties of the hydrophobically modified polyurethane core are conducive to improving the directional arrangement and glitter effect of the silver powder in the waterborne two-component silver powder paint, and can better solve the problems of sagging and poor silver powder orientation in the construction process of the existing waterborne two-component silver powder paint.

[0073] (3) The present invention adopts a monomer pre-emulsification process when preparing the water-based acrylate modified polyurethane dispersion. The role of adding part of the acrylate monomer and part of the initiator is to reduce the viscosity of the modified polyurethane and improve the success rate of phase inversion emulsification. It acts as both a solvent and a raw material for acrylic acid modification, avoiding the use of emulsifiers and improving the water resistance of the resin after film formation. DETAILED DESCRIPTION

[0074] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0075] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0076] The source information of the raw material components in the application examples of the present invention is as follows:

[0077] Wetting agent TEGO-245, purchased from Guangzhou Tianci New Materials Co., Ltd.;

[0078] Defoaming agent surfynol DF110D was purchased from Guangzhou Tianci New Materials Co., Ltd.;

[0079] Defoamer Surfynol 420, purchased from Guangzhou Tianci New Materials Co., Ltd.

[0080] Leveling agent BYK-333, purchased from Guangzhou Tianci New Materials Co., Ltd.;

[0081] Anti-flash rust agent NALZIN FA 179, purchased from Deqian (Shanghai) Chemical Co., Ltd.;

[0082] Silver powder SR-7010, purchased from Saier New Materials Company;

[0083] Dispersant BYK-190, purchased from Guangzhou Tianci New Materials Co., Ltd.;

[0084] PUR64, purchased from Mingling Chemical, Germany;

[0085] Coapur2025, purchased from Shanghai Lingrui Chemical Co., Ltd.;

[0086] Silver powder directional arrangement additive BYK-AQUATIX 8421 was purchased from Guangzhou Tianci New Materials Co., Ltd.;

[0087] Water-based isocyanate curing agent ultra 2655 was purchased from Covestro Polymers (China) Co., Ltd.

[0088] Example 1

[0089] A method for preparing a waterborne acrylate modified polyurethane dispersion comprises the following steps:

[0090] (1) Under the protection of dry nitrogen, the polyether polyol N210 (M n =1000) 60 parts, isophorone diisocyanate (IPDI) 18.34 parts are added into a four-necked flask, and 0.4 parts of dibutyltin dilaurate (T-12) catalyst is added, mixed evenly and heated to 85°C for reaction for 2 hours to obtain polyurethane prepolymer I; then the reaction system is cooled to 65°C, a mixed solution of acetone and methyl isobutyl ketone (10.12 parts of acetone and methyl isobutyl ketone) is used to dilute and reduce the viscosity of the polyurethane oligomer, and 0.2 parts of butyltin dilaurate (T-12) and 1.3 parts of diethylene glycol (DEG) are added to carry out chain extension reaction for 3 hours to obtain polyurethane prepolymer II;

[0091] (2) using 3.27 parts of linoleic acid (LA) and 1.53 parts of 2-hydroxyethyl methacrylate (HEMA) to end-cap the polyurethane prepolymer II with the terminal group of -NCO synthesized in step (1); that is, 0.2 parts of butyltin disilicate (T-12) was dissolved in 3.27 parts of 2-hydroxyethyl methacrylate (HEMA) and 1.53 parts of linoleic acid (LA) and added to the mixed solution of the polyurethane prepolymer II obtained in step (1), and the system temperature was increased to 75° C., and the mixture was reacted for 2.5 hours under stirring and nitrogen atmosphere, and then cooled to obtain a modified polyurethane;

[0092] (3) at 35° C., adding 1 / 3 of the total amount of acrylate monomers and initiators used for preparing an aqueous acrylate-modified polyurethane dispersion (i.e., 13.62 parts of methyl methacrylate, 13.33 parts of butyl acrylate (BA), 6.67 parts of isobornyl methacrylate (IBOMA), 5.67 parts of styrene (St), 1.31 parts of 2-hydroxyethyl methacrylate (HEMA), and 0.85 parts of azobisisobutyronitrile (AIBN)) to the modified polyurethane obtained in step (2), so that the acrylate monomers and the initiator are used as solvents to further dilute the modified polyurethane obtained in step (2); and neutralizing the modified polyurethane with 2.64 parts of triethylamine (TEA), and then, under high-speed stirring at a stirring speed of 800 rpm, dropwise adding 230.23 parts of deionized water to the modified polyurethane for phase inversion emulsification to obtain a milky white modified polyurethane mixed emulsion;

[0093] (4) Under the protection of inert gas nitrogen, the modified polyurethane mixed emulsion obtained in step (3) is heated to 75° C., and under stirring, a mixed solution of 26.38 parts of methyl methacrylate, 26.67 parts of butyl acrylate, 13.33 parts of isobornyl methacrylate, 11.33 parts of styrene, 2.63 parts of 2-hydroxyethyl methacrylate and 1.29 parts of azobisisobutyronitrile is slowly and dropwise added to the reaction system, and the dropping time is continued for 3 hours. After the dropping is completed, the mixture is kept warm for 2 hours, and then 1 part of potassium persulfate is dissolved in 10 parts of deionized water and added to the reaction system. The mixture is kept at a constant temperature of 75° C. for 1 hour and then cooled to room temperature to obtain a water-based acrylate modified polyurethane dispersion.

[0094] Example 2

[0095] A method for preparing a waterborne acrylate modified polyurethane dispersion comprises the following steps:

[0096] (1) Under the protection of dry nitrogen, the polyether polyol N210 (M n =1000) 60 parts, 4,4'-dicyclohexylmethane diisocyanate (HMDI) 20.46 parts are added into a four-necked flask, and 0.4 parts of dibutyltin dilaurate (T-12) catalyst is added, mixed evenly and heated to 85°C for reaction for 2 hours to obtain polyurethane prepolymer I; then the reaction system is cooled to 65°C, a mixed solution of acetone and methyl isobutyl ketone (10.12 parts of acetone and methyl isobutyl ketone) is used to dilute and reduce the viscosity of the polyurethane oligomer, and 0.2 parts of dibutyltin dilaurate (T-12) and 1.3 parts of diethylene glycol (DEG) are added to carry out chain extension reaction for 3 hours to obtain polyurethane prepolymer II;

[0097] (2) using 3.27 parts of linoleic acid (LA) and 1.53 parts of 2-hydroxyethyl methacrylate (HEMA) to end-cap the polyurethane prepolymer II with the terminal group of -NCO synthesized in step (1); that is, dissolving 0.2 parts of butyltin disilicate (T-12) in a mixed solution of 3.27 parts of 2-hydroxyethyl methacrylate (HEMA), 1.53 parts of linoleic acid (LA) and the polyurethane prepolymer II obtained in step (1), and raising the system temperature to 75° C., reacting for 2.5 hours under stirring and nitrogen atmosphere, and then cooling to obtain a modified polyurethane;

[0098] (3) at 35° C., adding 1 / 3 of the total amount of acrylate monomers and initiators used for preparing an aqueous acrylate-modified polyurethane dispersion (i.e., 16.44 parts of methyl methacrylate, 14.99 parts of butyl acrylate, 5 parts of isobornyl methacrylate, 3.34 parts of styrene, 1.26 parts of 2-hydroxyethyl methacrylate, and 0.85 parts of azobisisobutyronitrile) to the modified polyurethane obtained in step (2), so that the acrylate monomers and the initiator are used as solvents to further dilute the modified polyurethane obtained in step (2); and neutralizing the modified polyurethane with 2.64 parts of triethylamine (TEA), and then, under high-speed stirring at a stirring speed of 800 rpm, dropwise adding 246.35 parts of deionized water to the modified polyurethane for phase inversion emulsification, to obtain a milky white modified polyurethane mixed emulsion;

[0099] (4) Under the protection of inert gas nitrogen, the modified polyurethane mixed emulsion obtained in step (3) is heated to 75° C., and under stirring, a mixed solution of 32.89 parts of methyl methacrylate, 29.97 parts of butyl acrylate, 10 parts of isobornyl methacrylate, 6.67 parts of styrene, 2 parts of 2-hydroxyethyl methacrylate and 1.29 parts of azobisisobutyronitrile is slowly and dropwise added to the reaction system, and the dropping time lasts for 3 hours. After the dropping is completed, the mixture is kept warm for 2 hours, and then 1 part of potassium persulfate is dissolved in 10 parts of deionized water and added to the reaction system. The mixture is kept at a constant temperature of 75° C. for reaction for 1 hour and then cooled to room temperature to obtain a water-based acrylate modified polyurethane dispersion.

[0100] Example 3

[0101] A method for preparing a waterborne acrylate modified polyurethane dispersion comprises the following steps:

[0102] (1) Under the protection of dry nitrogen, the polyester polyol PCL (M n =1000) 60 parts, isophorone diisocyanate (IPDI) 18.34 parts are added into a four-necked flask, and 0.4 parts of dibutyltin dilaurate (T-12) catalyst is added, mixed evenly and heated to 85°C for reaction for 2 hours to obtain polyurethane prepolymer I; then the reaction system is cooled to 65°C, a mixed solution of acetone and methyl isobutyl ketone (10.12 parts of acetone and methyl isobutyl ketone) is used to dilute and reduce the viscosity of the polyurethane oligomer, and 0.2 parts of butyltin dilaurate (T-12) and 1.3 parts of diethylene glycol (DEG) are added to carry out chain extension reaction for 3 hours to obtain polyurethane prepolymer II;

[0103] (2) using 3.27 parts of linoleic acid (LA) and 1.53 parts of 2-hydroxyethyl methacrylate (HEMA) to end-cap the polyurethane prepolymer II with the terminal group of -NCO synthesized in step (1); that is, dissolving 0.2 parts of butyltin disilicate (T-12) in a mixed solution of 3.27 parts of 2-hydroxyethyl methacrylate (HEMA), 1.53 parts of linoleic acid (LA) and the polyurethane prepolymer II obtained in step (1), and raising the system temperature to 75° C., reacting for 2.5 hours under stirring and nitrogen atmosphere, and then cooling to obtain a modified polyurethane;

[0104] (3) at 35° C., adding 1 / 3 of the total amount of acrylate monomers and initiators used for preparing an aqueous acrylate-modified polyurethane dispersion (i.e., 13.62 parts of methyl methacrylate, 13.60 parts of butyl acrylate, 5.34 parts of isobornyl methacrylate, 4 parts of styrene, 1.33 parts of 2-hydroxyethyl methacrylate, and 0.85 parts of azobisisobutyronitrile) to the modified polyurethane obtained in step (2), so that the acrylate monomers and the initiator are used as solvents to further dilute the modified polyurethane obtained in step (2); and neutralizing the modified polyurethane with 2.64 parts of triethylamine (TEA), and then, under high-speed stirring at a stirring speed of 800 rpm, dropwise adding 234.65 parts of deionized water to the modified polyurethane for phase inversion emulsification to obtain a milky white modified polyurethane mixed emulsion;

[0105] (4) Under the protection of inert gas nitrogen, the modified polyurethane mixed emulsion obtained in step (3) is heated to 75°C, and under stirring, a mixed solution of 27.24 parts of methyl methacrylate, 27.19 parts of butyl acrylate, 8 parts of isobornyl methacrylate, 10.67 parts of styrene, 2.66 parts of 2-hydroxyethyl methacrylate and 1.29 parts of azobisisobutyronitrile is slowly and dropwise added to the reaction system, and the dropping time lasts for 3 hours. After the dropwise addition is completed, the temperature is kept for 2 hours, and then 1 part of potassium persulfate is dissolved in 10 parts of deionized water and added to the reaction system. The reaction is kept at a constant temperature of 75°C for 1 hour and then cooled to room temperature to obtain a water-based acrylate modified polyurethane dispersion.

[0106] Example 4

[0107] A method for preparing a waterborne acrylate modified polyurethane dispersion comprises the following steps:

[0108] (1) Under the protection of dry nitrogen, the polyester polyol PCL (M n=1000) 60 parts, 4,4'-dicyclohexylmethane diisocyanate (HMDI) 20.46 parts are added into a four-necked flask, and 0.4 parts of dibutyltin dilaurate (T-12) catalyst is added, mixed evenly and heated to 85°C for reaction for 2 hours to obtain polyurethane prepolymer I; then the reaction system is cooled to 65°C, a mixed solution of acetone and methyl isobutyl ketone (10.12 parts of acetone and methyl isobutyl ketone) is used to dilute and reduce the viscosity of the polyurethane oligomer, and 0.2 parts of dibutyltin dilaurate (T-12) and 1.3 parts of diethylene glycol (DEG) are added to carry out chain extension reaction for 3 hours to obtain polyurethane prepolymer II;

[0109] (2) using 3.27 parts of linoleic acid (LA) and 1.53 parts of 2-hydroxyethyl methacrylate (HEMA) to end-cap the polyurethane prepolymer II with the terminal group of -NCO synthesized in step (1); that is, dissolving 0.2 parts of butyltin disilicate (T-12) in a mixed solution of 3.27 parts of 2-hydroxyethyl methacrylate (HEMA), 1.53 parts of linoleic acid (LA) and the polyurethane prepolymer II obtained in step (1), and raising the system temperature to 75° C., reacting for 2.5 hours under stirring and nitrogen atmosphere, and then cooling to obtain a modified polyurethane;

[0110] (3) at 35° C., adding 1 / 3 of the total amount of acrylate monomers and initiators used for preparing an aqueous acrylate-modified polyurethane dispersion (i.e., 12.63 parts of methyl methacrylate, 15.64 parts of butyl acrylate, 4.44 parts of isobornyl methacrylate, 5.96 parts of styrene, 1.29 parts of 2-hydroxyethyl methacrylate, and 0.85 parts of azobisisobutyronitrile) to the modified polyurethane obtained in step (2), so that the acrylate monomers and the initiator are used as solvents to further dilute the modified polyurethane obtained in step (2); and neutralizing the modified polyurethane with 2.64 parts of triethylamine (TEA), and then, under high-speed stirring at a stirring speed of 800 rpm, dropwise adding 240.15 parts of deionized water to the modified polyurethane for phase inversion emulsification to obtain a milky white modified polyurethane mixed emulsion;

[0111] (4) Under the protection of inert gas nitrogen, the modified polyurethane mixed emulsion obtained in step (3) is heated to 75°C, and under stirring, a mixed solution of 25.25 parts of methyl methacrylate, 30.27 parts of butyl acrylate, 8.89 parts of isobornyl methacrylate, 11.93 parts of styrene, 2.57 parts of 2-hydroxyethyl methacrylate and 1.29 parts of azobisisobutyronitrile is slowly and dropwise added to the reaction system, and the dropping time lasts for 3 hours. After the dropwise addition is completed, the temperature is kept for 2 hours, and then 1 part of potassium persulfate is dissolved in 10 parts of deionized water and added to the reaction system. The reaction is kept at a constant temperature of 75°C for 1 hour and then cooled to room temperature to obtain a water-based acrylate modified polyurethane dispersion.

[0112] Example 5

[0113] A method for preparing a waterborne acrylate modified polyurethane dispersion comprises the following steps:

[0114] (1) In a three-necked flask equipped with a stirrer, a thermometer, and a reflux condenser, polyether polyol N210 (M) which had been vacuum dehydrated (vacuum dehydration for 1 h at a vacuum degree of 0.09 MPa and a temperature of 60°C) was added. n =1000) and 18.34 parts of isophorone diisocyanate (IPDI), and after adding 0.4 parts of dibutyltin dilaurate (T-12) in a three-necked flask, slowly heating to 85°C under stirring, constant temperature reaction for 2h to obtain polyurethane prepolymer I. After the constant temperature is completed, 3.5 parts of dimethylol propionic acid (DMPA) are added and reacted at 85°C for 1h to complete the chain extension reaction to obtain polyurethane prepolymer II;

[0115] (2) lowering the reaction temperature to 70° C., and adding 3.16 parts of n-octadecyl alcohol (C18), 1.53 parts of 2-hydroxyethyl methacrylate (HEMA) and 0.4 parts of dibutyltin dilaurate (T-12) to the polyurethane prepolymer II reaction system obtained in step (1) to carry out a capping reaction for 3 hours to obtain a modified polyurethane;

[0116] (3) cooling the temperature to room temperature, adding 1 / 3 of the total amount of acrylate monomers and initiators used for preparing the aqueous acrylate modified polyurethane dispersion (i.e., 11.21 parts of methyl methacrylate, 13.51 parts of butyl acrylate, 5.21 parts of isobornyl methacrylate, 5.96 parts of styrene, 1.15 parts of 2-hydroxyethyl methacrylate, and 0.85 parts of azobisisobutyronitrile) to the reaction system, using the acrylate monomers and initiators as solvents to further dilute the polyurethane prepolymer, and neutralizing the modified polyurethane with 2.64 parts of triethylamine (TEA), and then adding 225.65 parts of deionized water dropwise under high-speed stirring to emulsify the prepolymer by phase inversion, thereby obtaining a milky white modified polyurethane mixed emulsion;

[0117] (4) Under the protection of inert gas nitrogen, the modified polyurethane mixed emulsion obtained in step (3) is heated to 75° C., and under stirring, a mixed solution of 22.41 parts of methyl methacrylate, 27.03 parts of butyl acrylate, 10.43 parts of isobornyl methacrylate, 11.93 parts of styrene, 2.29 parts of 2-hydroxyethyl methacrylate and 1.94 parts of azobisisobutyronitrile is slowly and dropwise added to the reaction system, and the dropping time is continued for 3 hours. After the dropwise addition is completed, the reaction is continued at a constant temperature for 2 hours, and then a solution mixed with 1 part of potassium persulfate and 10 parts of deionized water is added to the reaction system, the temperature is raised to 85° C. and the reaction is carried out for 1.5 hours, and then the aqueous acrylate modified polyurethane dispersion is cooled to room temperature to obtain an aqueous acrylate modified polyurethane dispersion.

[0118] Comparative Example 1

[0119] The only difference between Comparative Example 1 and Example 5 is that in step (2) of Comparative Example 1, an equal amount of 2-hydroxyethyl methacrylate is used to replace n-octadecyl alcohol, that is, n-octadecyl alcohol is not added, and the amount of 2-hydroxyethyl methacrylate is 4.69 parts, and the rest is the same as Example 5.

[0120] Comparative Example 2

[0121] The difference between Comparative Example 2 and Example 5 is that in step (2) of Comparative Example 2, an equal amount of n-hexadecanol is used to replace the n-octadecyl alcohol in Example 5, and the rest is the same as Example 5.

[0122] Comparative Example 3

[0123] Comparative Example 3 uses an existing water-based acrylate-modified polyurethane dispersion, which is a water-based hydroxylated acrylic emulsion 154-E0324 purchased from Honeycomb Nanotechnology.

[0124] Comparative Example 4

[0125] Comparative Example 4 uses an existing water-based acrylate-modified polyurethane dispersion, water-based hydroxyl acrylic dispersion PA-4570 purchased from Guangzhou Guanzhi New Materials Co., Ltd.

[0126] Comparative Example 5

[0127] Comparative Example 5 uses an existing water-based acrylate-modified polyurethane dispersion, namely, water-based hydroxyl acrylic emulsion DB3730 purchased from Wuhan Double Bond New Materials Co., Ltd.

[0128] Comparative Example 6

[0129] Comparative Example 6 uses an existing water-based acrylate-modified polyurethane dispersion, namely, water-based hydroxylated acrylic dispersion AC-033B purchased from Ward Polymer Materials.

[0130] Application Example 1

[0131] A water-based two-component silver paint, comprising component A and component B, in parts by weight; wherein component A comprises 54 parts of the water-based acrylate modified polyurethane dispersion of Example 1, 4 parts of cosolvent dipropylene glycol butyl ether (DPNB), 1 part of cosolvent ethylene glycol butyl ether (BCS), 0.3 parts of neutralizer N,N-dimethylethanolamine (DMEA), 26 parts of deionized water, 0.2 parts of wetting agent TEGO-245, 0.2 parts of defoamer surfynol DF110D, 0.2 parts of defoamer Surfynol 420, 0.3 parts of leveling agent BYK-333, 0.8 parts of anti-flash rust agent NALZIN FA 179, 6 parts of silver powder SR-7010, and 0.5 parts of dispersant BYK-190;

[0132] Component B includes a water-based isocyanate curing agent ultra 2655 14 parts, propylene glycol methyl ether acetate (PMA) 5 parts.

[0133] A method for preparing a water-based two-component silver paint comprises the following steps:

[0134] (1) adding a water-based acrylate modified polyurethane dispersion to a paint mixing tank, adding a neutralizing agent N,N-dimethylethanolamine, a co-solvent dipropylene glycol butyl ether and ethylene glycol butyl ether in sequence under stirring at a speed of 600 rpm, and continuing to disperse for 5 minutes, and then adding a wetting agent, a defoaming agent, a leveling agent and an anti-flash rust agent to the paint mixing tank in sequence and dispersing for 5 minutes to obtain a mixed system;

[0135] (2) Add silver powder, deionized water and dispersant to another paint mixing tank, and slowly disperse at 200 rpm for 5 minutes to obtain the desired water-based silver powder slurry;

[0136] (3) At a stirring speed of 600 rpm, slowly add the water-based silver powder slurry prepared in step (2) to the mixed system of step (1), and continue to disperse for 20 minutes to obtain component A of the water-based two-component silver powder paint;

[0137] (4) Hydrophilic aliphatic polyisocyanate of hexamethylene diisocyanate HDI Ultra 2655 is dissolved in propylene glycol methyl ether acetate (PMA), and the mixture is mixed evenly to obtain component B of the water-based two-component silver paint.

[0138] During construction, components A and B are evenly mixed in a mass ratio of 7:1, and the mixture of components A and B is diluted in a dilution ratio of 25% to obtain a water-based two-component silver powder paint.

[0139] Application Example 2

[0140] The difference between Application Example 2 and Application Example 1 is that the water-based acrylate-modified polyurethane dispersion in Application Example 2 is the water-based acrylate-modified polyurethane dispersion prepared in Example 2, and the rest is the same as Application Example 1.

[0141] Application Example 3

[0142] The only difference between Application Example 3 and Application Example 1 is that the water-based acrylate-modified polyurethane dispersion in Application Example 3 is the water-based acrylate-modified polyurethane dispersion prepared in Example 3, and the rest is the same as Application Example 1.

[0143] Application Example 4

[0144] The difference between Application Example 4 and Application Example 1 is that the water-based acrylate-modified polyurethane dispersion in Application Example 4 is the water-based acrylate-modified polyurethane dispersion prepared in Example 4, and the rest is the same as Application Example 1.

[0145] Application Example 5

[0146] The only difference between Application Example 5 and Application Example 1 is that the water-based acrylate-modified polyurethane dispersion in Application Example 5 is the water-based acrylate-modified polyurethane dispersion prepared in Example 5, and the rest is the same as Application Example 1.

[0147] Application Example 6

[0148] The only difference between Application Example 6 and Application Example 1 is that component A in Application Example 6 also includes a rheological additive. PUR64 0.5 parts and Coapur2025 0.5 parts, and in step (1) of the preparation process, after adding the wetting agent, defoamer, leveling agent and anti-flash rust agent and dispersing for 5 minutes, the stirring speed is increased to 1200 rpm and the following are added in sequence: PUR64 and Coapur2025 were stirred for 5 minutes to obtain a mixed system, and the rest was the same as in Application Example 1.

[0149] Application Example 7

[0150] The only difference between Application Example 7 and Application Example 1 is that component A in Application Example 7 further includes 4.5 parts of a silver powder orientation aid BYK-AQUATIX 8421, and in step (1) of the preparation process, after adding the wetting agent, defoaming agent, leveling agent and anti-flash rust agent and dispersing for 5 minutes, the stirring speed is increased to 1200 rpm and the silver powder orientation aid is added, and stirred for 5 minutes to obtain a mixed system. The rest is the same as in Application Example 1.

[0151] Application Example 8

[0152] The only difference between Application Example 8 and Application Example 1 is that component A in Application Example 8 also includes 4.5 parts of magnesium aluminum silicate dispersion containing 20% ​​(mass fraction) of silver powder orientation aid, and in step (1) of the preparation process, after adding the wetting agent, defoaming agent, leveling agent and anti-flash rust agent and dispersing for 5 minutes, the stirring speed is increased to 1200 rpm and the silver powder orientation aid is added, and stirred for 5 minutes to obtain a mixed system. The rest is the same as Application Example 1.

[0153] Comparative application example 1

[0154] The only difference between Comparative Application Example 1 and Application Example 5 is that the water-based acrylate-modified polyurethane dispersion in Comparative Application Example 1 is the water-based acrylate-modified polyurethane dispersion prepared in Comparative Example 1, and the rest is the same as Application Example 5.

[0155] Comparative Application Example 2

[0156] The only difference between Comparative Application Example 2 and Application Example 5 is that the water-based acrylate-modified polyurethane dispersion in Comparative Application Example 2 is the water-based acrylate-modified polyurethane dispersion prepared in Comparative Example 2, and the rest is the same as Application Example 5.

[0157] Comparative Application Example 3

[0158] The only difference between Comparative Application Example 3 and Application Example 1 is that the water-based acrylate-modified polyurethane dispersion in Comparative Application Example 3 is the water-based acrylate-modified polyurethane dispersion of Comparative Example 3, and the rest is the same as Application Example 1.

[0159] Comparative Application Example 4

[0160] The only difference between Comparative Application Example 4 and Application Example 1 is that the water-based acrylate-modified polyurethane dispersion in Comparative Application Example 4 is the water-based acrylate-modified polyurethane dispersion prepared in Comparative Example 4, and the rest is the same as Application Example 1.

[0161] Comparative Application Example 5

[0162] The only difference between Comparative Application Example 5 and Application Example 1 is that the water-based acrylate-modified polyurethane dispersion in Comparative Application Example 5 is the water-based acrylate-modified polyurethane dispersion prepared in Comparative Example 5, and the rest is the same as Application Example 1.

[0163] Comparative Application Example 6

[0164] The only difference between Comparative Application Example 6 and Application Example 1 is that the water-based acrylate-modified polyurethane dispersion in Comparative Application Example 6 is the water-based acrylate-modified polyurethane dispersion prepared in Comparative Example 6, and the rest is the same as Application Example 1.

[0165] Performance Testing

[0166] 1. Physical performance test

[0167] The hydroxyl content, viscosity and solid content of the aqueous acrylate modified polyurethane dispersions of Examples 1-5 and Comparative Examples 1-6 were tested. The results are shown in Table 1.

[0168] Table 1: Test results of waterborne acrylate modified polyurethane dispersions of Examples 1-5 and Comparative Examples 1-6

[0169] Group Hydroxyl content (%) Viscosity (mPa·s) Solid content (%) Example 1 2.9 900 45±2 Example 2 2.9 960 45±2 Example 3 3.0 1080 45±2 Example 4 3.0 1190 45±2 Example 5 2.9 920 45±2 Comparative Example 1 2.9 540 45±2 Comparative Example 2 2.9 600 45±2 Comparative Example 3 3.0 200 40±2 Comparative Example 4 2.6 500 38±2 Comparative Example 5 3.2 300 40±2 Comparative Example 6 3.3 200 45±1

[0170] It can be seen from Table 1 that the viscosity of the waterborne acrylate modified polyurethane dispersion of the embodiment of the present invention is significantly higher than that of comparative examples 1-6, indicating that the resin molecular weight is relatively large, resulting in a high viscosity of the system. For silver powder paint, the larger the resin molecular weight, the more conducive it is to the arrangement of the silver powder.

[0171] 2. Performance test of water-based two-component silver paint

[0172] The substrate is tinplate. After pretreatment such as degreasing and grinding, the water-based two-component silver paint of Application Examples 1-8 and Comparative Example Application Examples 1-6 is sprayed onto the surface of the substrate by air spraying in a construction environment of 25±5°C and 65±5% RH. The drying time of the wet film is observed. After the surface is dry, the paint film is placed at 80°C and baked for 30 minutes to cure and cross-link to obtain a paint film with a film thickness of 20-25 μm. The paint film is then subjected to performance tests. The test items and test methods are as follows:

[0173] Drying time: refer to GB / T 1728-2020 (method B);

[0174] Gloss: Refer to GB / T 9754-2007;

[0175] Adhesion: refer to GB / T 9286-2021;

[0176] Water resistance: The cured paint film is cured at room temperature for 24 hours, and then the water resistance test is carried out according to GB / T 1733-1993;

[0177] Impact resistance: refer to GB / T 1732-2020;

[0178] Hardness: Refer to GB / T 6739-2006;

[0179] Flexibility: Refer to GB / T 1731-2020.

[0180] Application Examples 1-8 and Comparative Examples The performance test results of the silver powder paint coatings obtained by the water-based two-component silver powder paints of Application Examples 1-6 are shown in Table 2.

[0181] Table 2: Performance test results of the silver powder paint coating obtained by using the water-based two-component silver powder paint of Application Examples 1-8 and Comparative Examples 1-6

[0182]

[0183] As can be seen from Table 2, the paint films of the water-based two-component silver powder paint prepared by the water-based acrylate modified polyurethane dispersions of Examples 1-5 of the present invention have good gloss, adhesion, impact resistance, and water resistance, and can meet the application requirements of current industrial coatings for water-based two-component silver powder paints. After baking at 80°C for 30 minutes, the paint films all have excellent flexibility and initial hardness, which is conducive to the rapid stacking and transportation of the coated workpieces after they are off the production line.

[0184] The waterborne acrylate modified polyurethane dispersion in comparative application example 1 was not added with n-octadecyl alcohol during preparation, so the gloss, water resistance and impact resistance of the silver powder paint in comparative application example 1 were worse than those in application example 5. This indicates that the addition of n-octadecyl alcohol as a hydrophobic end-capping agent to modify the polyurethane prepolymer and synthesize a polyurethane with a hydrophobic end and a carbon-carbon double bond structure can improve the water resistance, gloss and impact resistance of the silver powder paint.

[0185] Comparative Application Example 2 uses an equal amount of n-hexadecyl alcohol to replace n-octadecyl alcohol, so that the gloss, water resistance and impact resistance of the silver powder paint in Comparative Application Example 2 are worse than those in Application Example 5. This shows that a specific type of end-capping agent must be added to modify the polyurethane prepolymer in order to improve the water resistance, gloss and impact resistance of the silver powder paint.

[0186] Comparative Examples 3-6 are all prepared by using water-based acrylate modified polyurethane dispersions in the prior art to prepare silver powder paints, so that the gloss, water resistance and impact resistance of the silver powder paints of Comparative Examples 3-6 are worse than those of Application Example 1, and the pencil hardness of Comparative Application Example 3-5 is lower than that of Application Example 1. It is explained that the present invention uses a hydrophobic end-capping agent to modify the polyurethane prepolymer to synthesize a polyurethane having a hydrophobic end and a carbon-carbon double bond structure, and then obtains a water-based acrylate modified polyurethane dispersion, which can improve the gloss, water resistance and impact resistance of the silver powder paint.

[0187] 3. Viscosity, thixotropy and flash index test of water-based two-component silver paint

[0188] The viscosity, thixotropy value and flash index of the water-based two-component silver powder paint of Example 1-8 and Comparative Example 1-6 were tested. The test method is as follows:

[0189] Viscosity: Detected using NDJ-1 rotational viscometer;

[0190] Thixotropic value: the viscosity ratio of water-based two-component silver paint at 60rpm and 6rpm on a rotational viscometer;

[0191] Flash index: Use SGY-A flash index measuring instrument to measure the paint film at 15°(L 15° )、45°(L 45° )、110°(L 110° ) The brightness values ​​at three angles are measured and calculated using the Flop index calculation formula:

[0192] Flop index = 2.69 × (L 15° -L 110° ) 1.11 / L 45° 0.86 .

[0193] The test results of viscosity, thixotropy value and flash index of the water-based two-component silver powder paint of Application Examples 1-8 and Comparative Examples 1-6 are shown in Table 3.

[0194] Table 3: Viscosity, thixotropy and flash index test results of water-based two-component silver paint of Application Examples 1-8 and Comparative Examples 1-6

[0195]

[0196] It can be seen from Table 3 that the water-based two-component silver powder paint of Application Examples 1-8 of the present invention has good viscosity, thixotropic value and flash index, indicating that the water-based acrylate modified polyurethane dispersion prepared by Examples 1-5 of the present invention can improve the thixotropic value and flash index of the silver powder paint.

[0197] From the results of Application Examples 6-8 and Application Example 1, it can be seen that the rheological additive in Application Example 6 The use of PUR 64 and Coapur2025 has limited effect on the silver powder orientation effect and cannot improve the silver powder paint film flash index. However, the use of silver powder orientation additive BYK-AQUATIX 8421 (modified ethylene-vinyl acetate copolymer wax rheology modified wax emulsion) and magnesium aluminum silicate dispersion can significantly improve the thixotropy and silver powder orientation effect of water-based two-component silver powder paint. In view of the cost of coating formulation, magnesium aluminum silicate dispersion can be used as a cheap substitute for silver powder orientation additive BYK-AQUATIX 8421 under the same conditions.

[0198] The only difference between Comparative Application Example 1 and Application Example 5 is that in Comparative Application Example 1, n-octadecyl alcohol was not used to modify the polyurethane prepolymer during the preparation of the water-based acrylate-modified polyurethane dispersion, so that the thixotropic value and flash index of the silver powder paint prepared in Comparative Application Example 1 are significantly lower than those in Application Example 5, indicating that the water-based acrylate-modified polyurethane dispersion obtained by modifying the polyurethane prepolymer with the blocking agent n-octadecyl alcohol can be applied to silver powder paint, which can significantly improve the thixotropic value and flash index of the silver powder paint.

[0199] The only difference between Comparative Application Example 2 and Application Example 5 is that Comparative Application Example 2 uses an equal amount of n-hexadecyl alcohol to replace n-octadecyl alcohol, so that the thixotropic value and flash index of the silver powder paint prepared in Comparative Application Example 2 are significantly lower than those in Application Example 5, indicating that the water-based acrylate modified polyurethane dispersion obtained by modifying the polyurethane prepolymer with the blocking agent n-octadecyl alcohol can be applied to silver powder paint, which can significantly improve the thixotropic value and flash index of the silver powder paint.

[0200] It can be seen from the test results of comparative application examples 1 and 2 that the present invention needs to use a specific capping agent (octadecyl alcohol or linoleic acid) in the process of preparing the water-based acrylate-modified polyurethane dispersion in order to better improve the thickening and thixotropy of the water-based acrylate-modified polyurethane dispersion, thereby improving the thixotropic value and flash index of the silver powder paint.

[0201] Comparative Application Examples 3-6 all use existing waterborne acrylate modified polyurethane dispersions, and the thixotropic value and flash index of the silver powder paint prepared in Comparative Application Examples 3-6 are significantly lower than the thixotropic value and flash index of the silver powder paint in Application Example 1 of the present invention. This indicates that the waterborne acrylate modified polyurethane dispersion with a specific structure prepared in the present invention can improve the thixotropic value and flash index of the silver powder paint.

[0202] In summary, the present invention uses a hydrophobic end-capping agent (octadecyl alcohol and / or linoleic acid) to modify a polyurethane prepolymer, synthesizes a modified polyurethane resin having a hydrophobic end and a carbon-carbon double bond structure, and uses the hydrophobic modified polyurethane as a core, and through a free radical polymerization reaction, polyacrylate is grafted on the core to synthesize a water-based acrylate modified polyurethane having a core-shell structure. The modified polyurethane with a hydrophobic end is further linked by hydrogen bonds between the hydrophilic segments of the polyurethane core and the polyacrylate shell layer to form a transient grid structure, thereby generating a thickening phenomenon and thixotropic properties, which is beneficial to improving the directional arrangement and flashing effect of the silver powder in the water-based two-component silver powder paint, and can better solve the problems of sagging and poor orientation of the silver powder in the construction process of the existing water-based two-component silver powder paint, and can improve water resistance and mechanical properties.

[0203] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A water-based acrylate-modified polyurethane dispersion, characterized in that: The aqueous acrylate modified polyurethane dispersion has a core-shell structure; the core of the core-shell structure comprises modified polyurethane; the shell layer of the core-shell structure comprises polyacrylate; The modified polyurethane is obtained by modifying the polyurethane prepolymer with the end-capping agent 1; The end-capping agent 1 includes at least one of linoleic acid and n-octadecyl alcohol.

2. The aqueous acrylate-modified polyurethane dispersion according to claim 1, characterized in that: The preparation method of the modified polyurethane comprises the following steps: (1) vacuum dehydrating the polymer polyol, adding catalyst 1 and isocyanate monomer, and carrying out reaction 1 to obtain polyurethane prepolymer I; adding catalyst 2 and chain extender to the polyurethane prepolymer I, and carrying out reaction 2 to obtain polyurethane prepolymer II; (2) The end-capping agent 1, the end-capping agent 2 and the polyurethane prepolymer II obtained in step (1) are mixed and reacted with each other to obtain the modified polyurethane.

3. The aqueous acrylate-modified polyurethane dispersion according to claim 2, characterized in that: In step (1), the polymer polyol includes at least one of polyether polyol and polyester polyol; and / or, the catalyst 1 and the catalyst 2 both include dibutyltin dilaurate; and / or, the isocyanate monomer includes at least one of isophorone diisocyanate and 4,4'-dicyclohexylmethane diisocyanate; and / or, the chain extender includes at least one of diethylene glycol, dihydroxymethylpropionic acid, and 1,4-butanediol-2-sodium sulfonate.

4. The aqueous acrylate-modified polyurethane dispersion according to claim 2, characterized in that: In step (2), the end-capping agent 1 includes at least one of linoleic acid and n-octadecyl alcohol; and / or the end-capping agent 2 includes 2-hydroxyethyl methacrylate.

5. The aqueous acrylate-modified polyurethane dispersion according to claim 2, characterized in that: In step (1), the reaction temperature of reaction 1 is 75-90° C., and the reaction time of reaction 1 is 1.5-2.5 h; and / or the reaction temperature of reaction 2 is 55-75° C., and the reaction time of reaction 2 is 2.5-3.5 h; And / or, in step (2), the reaction temperature of reaction 3 is 65-85°C, and the reaction time of reaction 3 is 2.0-3.0h.

6. The method for preparing the aqueous acrylate-modified polyurethane dispersion according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing an acrylate monomer and an initiator to obtain a mixture, taking a portion of the mixture and mixing it with a modified polyurethane and a neutralizer, and emulsifying to obtain a mixed emulsion; (2) mixing the remaining mixture with the mixed emulsion obtained in step (1), reacting the mixture, and obtaining the water-based acrylate-modified polyurethane dispersion.

7. The preparation method according to claim 6, characterized in that: The acrylic ester monomer includes at least one of methacrylic acid, isobornyl methacrylate, isobutyl methacrylate, glycidyl methacrylate, isooctyl methacrylate, methyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, acrylic acid, n-butyl acrylate, acrylamide, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, cyclohexyl acrylate, styrene, and isobornyl acrylate; and / or, the initiator includes at least one of tert-butyl perbenzoate, di-tert-butyl peroxide, azobisisobutyronitrile, di-tert-amyl peroxide, potassium persulfate, ammonium persulfate, and sodium persulfate; and / or, the neutralizer includes an amine neutralizer.

8. The preparation method according to claim 6, characterized in that: In step (2), the reaction temperature is 65-85° C., and the reaction time is 1.5-2.5 h.

9. A silver powder paint, characterized in that: The invention comprises the aqueous acrylate modified polyurethane dispersion according to any one of claims 1 to 5.

10. The silver powder paint according to claim 9, characterized in that: The invention comprises component A and component B; the component A comprises waterborne acrylate modified polyurethane dispersion, cosolvent A and silver powder; the component B comprises isocyanate curing agent and cosolvent B.

Citation Information

Patent Citations

  • Polyurethane-acrylic ester composite emulsion of core-shell interpenetrating polymer network structure and preparation method thereof

    CN105175661A

  • Waterborne polyurethane / acrylate composite emulsion for single-component plastic silver powder paint and preparation method thereof

    CN112321774A

  • Combined rheology modifier, preparation method and application thereof

    CN113072832A

  • Water-based coating composition and method for forming multilayer coating film using said composition

    CN113874447A

  • Core-shell polymeric materials

    US20140275395A1

Cited By

  • Water-based automobile silver powder paint with high brightness and high fine and smooth feeling as well as preparation method and application of water-based automobile silver powder paint

    CN120059552A