Protective coating as well as preparation method and application thereof in chemical milling in aircraft industry

By using protective coatings prepared by components such as formaldehyde and polymers of ammonia and ethane chloride, the problem of high solvent toxicity in the prior art is solved, and a coating with high elasticity and heat resistance acid and alkali resistance is achieved, which is in line with the national defense science industry Technical Committee standards and reduces impacts on the environment and workers' health.

CN118931308AActive Publication Date: 2024-11-12LUHOPE ADVANCED MATERIALS TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411174578.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The solvent used in existing chemical milling protective coatings is highly toxic and affects the environment and workers' health.

Method used

Polymers of formaldehyde, ammonia and ethane chloride, N-[(5-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine and 1,3,5-triglycidyl-S- Components such as triazine trione form amino resins of polymerization through ring-opening polymerization. Combined with D20 solvent oil and propylene glycol methyl ether acetate as composite solvents, a new protective coating is prepared with high elasticity and heat-resistant acids. Alkaline chemical milling liquid performance.

Benefits of technology

The protective coating has high elasticity, heat-resistant acid and alkali chemical milling liquid properties. The coating is easy to peel off manually and is not easy to break. It complies with the standards of the National Defense Science and Industry Technical Committee and does not contain halogenated hydrocarbons and toluene, reducing the environmental and workers' health. Influence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010359980000091
    Figure BDA0005010359980000091
  • Figure BDA0005010359980000101
    Figure BDA0005010359980000101
  • Figure BDA0005010359980000111
    Figure BDA0005010359980000111
Patent Text Reader

Abstract

The invention discloses a protective coating as well as a preparation method and application thereof in chemical milling in the aircraft industry. The protective coating comprises a component A and a component B, the component A is prepared from the following components in percentage by mass: 30 to 40 percent of a polymer of formaldehyde, ammonia and chloroethane, 1 to 2 percent of N-[(5-methyl-1H-benzotriazole-1-yl) methyl] diethanol amine and 58 to 69 percent of a composite solvent; the composite solvent comprises D20 solvent oil and propylene glycol methyl ether acetate, and the mass ratio of the D20 solvent oil to the propylene glycol methyl ether acetate is 4: (1-1.5); the component B is 1, 3, 5-triglycidol-S-triazinetrione, and the component B is an organic solvent; the volume ratio of the component A to the component B is 10: (1-3). A coating obtained after construction of the protective paint has the performance of high elasticity and resistance to heat acid and alkali chemical milling liquid, has a good protective effect on metal, can be stripped manually, is not prone to breakage, and meets the national defense science industrial technology committee standard HB 5453-2004 aluminum alloy chemical milling protective paint specification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a protective coating and a preparation method thereof and application thereof in chemical milling in the aviation industry. Background Art

[0002] In the aviation manufacturing industry, titanium alloy, aluminum alloy, magnesium alloy, steel and other metal sheet materials are chemically milled into designed patterns, and protective coatings are needed to protect the parts that do not require chemical milling. During construction, the protective coating is applied to the metal sheet material, and a protective film is formed after drying, and the protective coating is peeled off after completion. Therefore, the protective coating is required to be acid and alkali resistant, have good toughness and elongation at break, and be easy to peel off manually after completion. At present, the market mainly uses foreign protective coatings, such as AC-850, AC-828, etc., but the solvents used in these protective coatings are tetrachloroethylene and toluene, which have a relatively large impact on the environment and workers' health.

[0003] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a protective coating and a preparation method thereof and its application in chemical milling in the aviation industry, aiming to solve the problem of high toxicity of solvents used in existing chemical milling protective coatings.

[0005] The technical solution of the present invention is as follows:

[0006] In a first aspect of the present invention, a protective coating is provided, the protective coating comprising component A and component B;

[0007] The component A comprises, by mass percentage:

[0008] Formaldehyde polymer with ammonia and ethyl chloride 30-40%;

[0009] N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine 1-2%;

[0010] Composite solvent 58-69%;

[0011] The composite solvent comprises D20 solvent oil and propylene glycol methyl ether acetate, and the mass ratio of the D20 solvent oil to propylene glycol methyl ether acetate is 4:(1-1.5);

[0012] The B component is 1,3,5-triglycidyl-S-triazinetrione;

[0013] The volume ratio of the component A to the component B is 10:(1-3).

[0014] The second aspect of the present invention provides a method for preparing the protective coating as described in the first aspect, comprising:

[0015] Add a composite solvent, a polymer of formaldehyde, ammonia and ethyl chloride, and N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine into a reaction container according to mass percentage, and stir until the mixture is uniform to obtain component A;

[0016] 1,3,5-triglycidyl-S-triazinetrione was added according to the volume ratio to obtain component B.

[0017] According to a preferred technical solution, the stirring speed is 60 to 120 rpm, and the stirring time is 20 to 30 minutes.

[0018] The third aspect of the present invention provides an application of a protective coating in chemical milling in the aviation industry, wherein the protective coating as described in the first aspect or the protective coating prepared by the preparation method described in the second aspect is applied to the surface protection of metal materials in chemical milling in the aviation industry.

[0019] The preferred technical solution is a method for using the protective coating in chemical milling in the aviation industry, comprising the steps of:

[0020] The component A and the component B are mixed uniformly according to a volume ratio to obtain a mixed protective coating;

[0021] The mixed protective coating is left to stand for 10 to 20 minutes and then transferred to the metal material and dried to form a coating with a protective effect.

[0022] According to a preferred technical solution, the transfer process is selected from one of spraying, painting and brushing.

[0023] According to a preferred technical solution, the metal material is selected from titanium alloy, aluminum alloy, magnesium alloy and steel.

[0024] According to a preferred technical solution, the drying temperature is 10 to 40° C., and the drying time is 6 to 24 hours.

[0025] Beneficial effects: The protective coating of the present invention uses D20 solvent oil and propylene glycol methyl ether acetate as composite solvents, and polymerizes the polymer of formaldehyde, ammonia and ethyl chloride and 1,3,5-triglycidyl-S-triazinetrione into a high-molecular amino resin through a ring-opening polymerization reaction, and N-[(5-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine is added thereto as a corrosion inhibitor. The coating obtained after the construction of the protective coating has the properties of high elasticity and resistance to heat, acid and alkali chemical milling liquids, has a good protective effect on metals, and the coating can be manually peeled off and is not easy to break, which complies with the National Defense Science and Technology Committee Standard HB5453-2004 Aluminum Alloy Chemical Milling Protective Coating Specification. Compared with the prior art, the composite solvent in the protective coating of the present invention does not contain halogenated hydrocarbons and toluene, has less impact on the environment and workers' health, and can be applied to large-scale production. DETAILED DESCRIPTION

[0026] The present invention provides a protective coating and a preparation method thereof and application in chemical milling in the aviation industry. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below.

[0027] An embodiment of the present invention provides a protective coating, the protective coating comprising component A and component B;

[0028] The component A comprises, by mass percentage:

[0029] Formaldehyde polymer with ammonia and ethyl chloride 30-40%;

[0030] N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine 1-2%;

[0031] Composite solvent 58-69%;

[0032] The composite solvent comprises D20 solvent oil and propylene glycol methyl ether acetate, and the mass ratio of the D20 solvent oil to propylene glycol methyl ether acetate is 4:(1-1.5);

[0033] The B component is 1,3,5-triglycidyl-S-triazinetrione;

[0034] The volume ratio of the component A to the component B is 10:(1-3).

[0035] Specifically, the polymer of formaldehyde, ammonia and ethyl chloride (CAS No.: 63512-71-0) of component A is polymerized by formaldehyde, ammonia and ethyl chloride in a molar ratio of 1:1:1, and is a low polymer rich in amino groups. The polymer of formaldehyde, ammonia and ethyl chloride used in the following specific examples 1 to 2 and comparative examples 1 to 4 is a polymer of Chemtura, Inc. Base, but not limited to this. The structural formula of 1,3,5-triglycidyl-S-triazinetrione (CAS No.: 2451-62-9) of component B is: The structure contains three epoxy groups, and the amino groups of the polymer of formaldehyde, ammonia and ethyl chloride produce a ring-opening polymerization reaction at room temperature to achieve molecular weight growth and polymerize into a high-molecular amino resin. After the solvent evaporates, a dry coating with high elasticity and toughness that can be peeled off by hand is formed to protect the metal.

[0036] The structural formula of N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine (CAS No.: 80584-88-9) of component A is: It is an effective metal corrosion inhibitor. Its mechanism is to adsorb or coordinate with metal ions on the metal surface to form a protective film that blocks corrosive liquids. Its effect is better than the commonly used metal slow-release agent benzotriazole.

[0037] The composite solvent of component A includes D20 solvent oil and propylene glycol methyl ether acetate (CAS No.: 108-65-6), wherein D20 solvent oil, also known as D20, is a dearomatized hydrogenated alkane solvent with a closed cup flash point of 20 to 30° C. The D20 solvent oil used in the following specific examples 1 to 2 and comparative examples 1 to 4 is a product of Maoming Branch of China Petrochemical Corporation, but is not limited thereto. When the composite solvent of component A is all D20 solvent oil, the viscosity of component A and component B after mixing is the highest, the solution is turbid, easy to stratify, and the coating is not easy to level and defoam; when the composite solvent of component A is all propylene glycol methyl ether acetate, the viscosity of component A and component B after mixing is the lowest, which is not conducive to forming a coating of appropriate thickness on a vertical workpiece and will increase the number of coatings; when the mass ratio of D20 solvent oil and propylene glycol methyl ether acetate in the composite solvent of component A is 4: (1-1.5), component A and component B have appropriate viscosity after mixing, are stable in storage, can be used directly without dilution, have good leveling performance and rapid defoaming performance, and can form a coating of appropriate thickness on a vertical workpiece.

[0038] Component A and component B are mixed in a volume ratio of 10:(1-3), and after curing, the coating has an etching ratio of <1.1 (an indicator of the protective metal of the chemical milling protective coating. The larger this number is, the larger the size of the corrosive liquid invading the boundary to the protective area during chemical milling. The HB 5453-2004 standard requires 0.9-1.1), and has a tensile elongation of >750%. Therefore, the coating formed by the protective coating of the present invention is easy to peel off manually and is not easy to break. Among them, when the proportion of 1,3,5-triglycidyl-S-triazinetrione increases, there is a lower etching ratio, but the difficulty of peeling increases and the adhesion is large; when the proportion of 1,3,5-triglycidyl-S-triazinetrione decreases, the etching ratio increases, which is not conducive to protection, and the adhesion also becomes lower.

[0039] The embodiment of the present invention also provides a method for preparing the protective coating as described above, comprising:

[0040] Add a composite solvent, a polymer of formaldehyde, ammonia and ethyl chloride, and N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine into a reaction container according to mass percentage, and stir until the mixture is uniform to obtain component A;

[0041] 1,3,5-triglycidyl-S-triazinetrione was added according to the volume ratio to obtain component B.

[0042] In some embodiments, the stirring speed is 60 to 120 rpm, and the stirring time is 20 to 30 minutes.

[0043] An embodiment of the present invention further provides an application of a protective coating in chemical milling in the aviation industry, wherein the protective coating as described above or the protective coating prepared by the preparation method as described above is applied to the surface protection of metal materials in chemical milling in the aviation industry.

[0044] In some embodiments, the method of using the protective coating in chemical milling in the aviation industry comprises the steps of:

[0045] The component A and the component B are mixed uniformly according to a volume ratio to obtain a mixed protective coating;

[0046] The mixed protective coating is left to stand for 10 to 20 minutes and then transferred to the metal material and dried to form a coating with a protective effect.

[0047] In some embodiments, the transfer process is selected from one of spraying, painting, and brushing.

[0048] In some embodiments, the metal material is selected from titanium alloy, aluminum alloy, magnesium alloy, and steel.

[0049] In some embodiments, the drying temperature is 10 to 40° C., and the drying time is 6 to 24 hours.

[0050] In a specific embodiment, during construction, component A and component B are mixed in a volume ratio of 10: (1-3), and allowed to stand for 10-20 minutes before use. The sheet metal material can be sprayed, coated, or brushed for construction. The surface is dried at room temperature for about 30-60 minutes, and is completely dry after 6-8 hours to form a layer of highly elastic, corrosion-resistant metal protective coating. After the sheet metal material is cut into a specified shape in the chemical milling area, the coating of the part to be corroded can be manually stripped off and placed in the liquid tank of the chemical milling area for chemical milling. The part of the sheet metal material where the coating is not stripped off is protected by the coating and is not corroded by the chemical milling liquid.

[0051] The present invention will be further described below by means of specific examples.

[0052] Example 1

[0053] This embodiment provides a protective coating, which specifically includes:

[0054] Component A:

[0055] Formaldehyde, polymer with ammonia and ethyl chloride 30%;

[0056] N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine 1%;

[0057] Composite solvent 69%;

[0058] The composite solvent is D20 solvent oil and propylene glycol methyl ether acetate in a mass ratio of 4:1;

[0059] Component B:

[0060] 1,3,5-triglycidyl-S-triazinetrione;

[0061] The volume ratio of component A to component B is 10:1.

[0062] The preparation method of component A is as follows: a composite solvent, a polymer of formaldehyde, ammonia and ethyl chloride (commercially available), and N-[(5-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine (commercially available) are added into a stirring tank according to mass percentage, stirring is started at a speed of 120 minutes / revolution, stirring is stopped after 25 minutes, and the mixture is allowed to stand for 30 minutes before filling.

[0063] The preparation method of component B is as follows: 1,3,5-triglycidyl-S-triazinetrione (commercially available) is directly packaged.

[0064] During construction, mix component A and component B evenly and let them stand for 15 minutes before use.

[0065] Example 2

[0066] This embodiment provides a protective coating, which specifically includes:

[0067] Component A:

[0068] Formaldehyde, polymer with ammonia and ethyl chloride 40%;

[0069] N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine 2%;

[0070] Composite solvent 58%;

[0071] The composite solvent is D20 solvent oil and propylene glycol methyl ether acetate in a mass ratio of 4:1.5;

[0072] Component B:

[0073] 1,3,5-triglycidyl-S-triazinetrione;

[0074] The volume ratio of component A to component B is 10:3.

[0075] The preparation method of component A is as follows: a composite solvent, a polymer of formaldehyde, ammonia and ethyl chloride (commercially available), and N-[(5-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine (commercially available) are added into a stirring tank according to mass percentage, stirring is started at a speed of 60 minutes / revolution, stirring is stopped after 25 minutes, and the mixture is allowed to stand for 30 minutes before filling.

[0076] The preparation method of component B is as follows: 1,3,5-triglycidyl-S-triazinetrione (commercially available) is directly packaged.

[0077] During construction, mix component A and component B evenly and let them stand for 15 minutes before use.

[0078] Comparative Example 1

[0079] This comparative example provides a comparative protective coating, which differs from Example 1 only in that 1% of N-[(5-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine in component A is replaced with 1% of benzotriazole (commercially available), and the remaining components and preparation methods are the same.

[0080] Comparative Example 2

[0081] This comparative example provides a comparative protective coating, which differs from Example 1 only in that the volume ratio of component A to component B is changed from 10:1 to 10:0.5, and the remaining components and preparation methods are the same.

[0082] Comparative Example 3

[0083] This comparative example provides a comparative protective coating, which differs from Example 1 only in that the volume ratio of component A to component B is changed from 10:1 to 10:3, and the remaining components and preparation methods are the same.

[0084] Comparative Example 4

[0085] This comparative example provides a comparative protective coating, which differs from Example 1 only in that the volume ratio of component A to component B is changed from 10:1 to 10:4, and the remaining components and preparation methods are the same.

[0086] Performance Testing

[0087] (1) Effect of sustained-release agent type on sustained-release effect

[0088] The protective coating of Example 1 and the comparative protective coating of Comparative Example 1 were respectively applied to 2A12 T4 aluminum alloy plates, dried for 24 hours, and then immersed in an acid-base liquid at 90°C-95°C. The specific method was based on HB 5453-2004, and the aluminum alloy corrosion-free time was recorded. The test results are shown in the following table.

[0089]

[0090] As can be seen from the above table, compared with the comparative protective coating in comparative example 1 using benzotriazole as the corrosion inhibitor, the protective coating in Example 1 using N-[(5-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine as the corrosion inhibitor has a longer acid and alkali resistance retention time, and the corrosion inhibition effect is improved, which meets the National Defense Science and Technology Committee Standard HB5453-2004 Aluminum Alloy Chemical Milling Protective Coating Specification (acid resistance for 30 minutes, alkali resistance for 8 hours). However, the comparative protective coating in comparative example 1 does not meet the technical requirements of HB 5453-2004.

[0091] (2) Effect of the volume ratio of component A and component B on the etching ratio

[0092] The protective coating of Example 1 and the comparative protective coatings of Comparative Examples 2 to 4 were coated on 2A12 T4 aluminum alloy plates, dried for 24 hours, and then immersed in an acid-base liquid at 90°C-95°C. The specific method was based on HB 5453-2004, and the etching ratio and peel strength values ​​were recorded. The test results are shown in the following table.

[0093] Comparative Example 2 Example 1 Comparative Example 3 Comparative Example 4 Volume ratio of component A to component B 10:0.5 10:1 10:3 10:4 Etching ratio 1.6 1.0 0.9 0.7 Peel strength N / m 210 332 557 707

[0094] It can be seen from the above table that the higher the content of component B, the smaller the etching ratio, the greater the adhesion and the greater the difficulty of stripping.

[0095] (3) Physical and chemical index tests of Example 1 and Example 2

[0096] According to the National Defense Science and Technology Committee Standard HB 5453-2004 Specification for Aluminum Alloy Chemical Milling Protective Coating, the physical and chemical indicators of Example 1 and Example 2 were tested, and the test results are shown in the following table.

[0097]

[0098]

[0099] It can be seen from the above table that the protective coatings of Example 1 and Example 2 meet the technical requirements of milling coatings in the aviation industry.

[0100] In summary, the present invention provides a protective coating and a preparation method thereof and its application in chemical milling in the aviation industry. The protective coating comprises component A and component B; the component A comprises, by mass percentage, 30-40% of a polymer of formaldehyde, ammonia and ethyl chloride, 1-2% of N-[(5-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, and 58-69% of a composite solvent; the composite solvent comprises D20 solvent oil and propylene glycol methyl ether acetate, and the mass ratio of the D20 solvent oil to the propylene glycol methyl ether acetate is 4:(1-1.5); the component B is 1,3,5-triglycidyl-S-triazinetrione; the volume ratio of the component A to the component B is 10:(1-3). The coating obtained after the protective coating of the present invention is applied has the properties of high elasticity and resistance to heat, acid and alkali chemical milling liquid, has a good protective effect on metals, and the coating can be peeled off manually and is not easy to break, and meets the standard HB 5453-2004 of the National Defense Science and Technology Committee for aluminum alloy chemical milling protective coating specifications. At the same time, the protective coating does not contain halogenated hydrocarbons and toluene, has little impact on the environment and workers' health, and can be applied to large-scale production.

[0101] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A protective coating, characterized in that: The protective coating comprises component A and component B; The component A comprises, by mass percentage: Formaldehyde polymer with ammonia and ethyl chloride 30-40%; N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine 1-2%; Composite solvent 58-69%; The composite solvent comprises D20 solvent oil and propylene glycol methyl ether acetate, and the mass ratio of the D20 solvent oil to propylene glycol methyl ether acetate is 4:(1-1.5); The B component is 1,3,5-triglycidyl-S-triazinetrione; The volume ratio of the component A to the component B is 10:(1-3).

2. A method for preparing the protective coating according to claim 1, characterized in that: include: Add a composite solvent, a polymer of formaldehyde, ammonia and ethyl chloride, and N-[(5-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine into a reaction container according to mass percentage, and stir until the mixture is uniform to obtain component A; 1,3,5-triglycidyl-S-triazinetrione was added according to the volume ratio to obtain component B.

3. The preparation method according to claim 2, characterized in that: The stirring speed is 60 to 120 revolutions per minute, and the stirring time is 20 to 30 minutes.

4. Application of a protective coating in chemical milling in the aviation industry, characterized in that: The protective coating as claimed in claim 1 or the protective coating prepared by the preparation method as claimed in any one of claims 2 to 3 is applied to the surface protection of metal materials in chemical milling in the aviation industry.

5. The use according to claim 4, characterized in that: The method for using the protective coating in chemical milling in the aviation industry comprises the steps of: The component A and the component B are mixed uniformly according to a volume ratio to obtain a mixed protective coating; The mixed protective coating is left to stand for 10 to 20 minutes and then transferred to the metal material and dried to form a coating with a protective effect.

6. The use according to claim 5, characterized in that: The transfer process is selected from one of spraying, coating and brushing.

7. The use according to claim 5, characterized in that: The metal material is selected from titanium alloy, aluminum alloy, magnesium alloy and steel.

8. The use according to claim 5, characterized in that: The drying temperature is 10 to 40° C., and the drying time is 6 to 24 hours.

Citation Information

Patent Citations

  • High-performance chemical milling protective paint and preparation method thereof

    CN104073073A

  • Solvent type chemical milling protective coating and preparation method thereof

    CN116004075A

  • Anti-settling chemical milling protective strippable coating

    CN117467324A

  • Dry Primer Film Composite and Use Thereof

    US20160023243A1