Self-early-warning anticorrosive paint, anticorrosive coating and application thereof in corrosion prevention of metal materials

Through layered spraying technology of modified zirconium phosphate and tannin-loaded silica microcapsules, a layered structural coating is formed, which solves the anticorrosion performance problems caused by micropores and defects of the anticorrosion coating, and achieves long-term anticorrosion and self-contained The early warning function significantly improves the corrosion resistance of metal materials.

CN118931327AActive Publication Date: 2024-11-12BEIJING SINOPERM TECH

Patent Information

Application Number
CN202411251196.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-12
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The micropores and defects formed during the curing process of existing anticorrosion coatings lead to poor anticorrosion performance, unsatisfactory long-term anticorrosion performance, unable to determine the internal corrosion location, and lack of corrosion warning and long-term anticorrosion multifunctional coatings.

Method used

Using layered spraying technology of silica microcapsules with modified zirconium phosphate and loaded tanninic acid, the physical shielding performance of zirconium phosphate and the corrosion-inhibiting self-warning function of silica microcapsules is used to form a layered structural coating to realize physical Barrier and chemical repair.

Benefits of technology

It significantly improves the long-term anti-corrosion performance of the coating, can maintain high impedance modulus under high temperature and high salt conditions, and can realize early warning and repair of internal corrosion areas through color changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931327A_ABST
    Figure CN118931327A_ABST
Patent Text Reader

Abstract

The invention provides a self-early-warning anticorrosive paint, an anticorrosive coating and application thereof. The self-early-warning anticorrosive paint comprises a first paint and a second paint, wherein the first paint comprises modified zirconium phosphate and a coating matrix; the second coating comprises a silicon dioxide microcapsule and a coating matrix; the modified zirconium phosphate is prepared by modifying zirconium phosphate by using a modifier; the silicon dioxide microcapsule is prepared by impregnating mesoporous silicon dioxide with tannic acid so that tannic acid is loaded inside the silicon dioxide microcapsule. The invention also provides a method for carrying out anti-corrosion treatment on a metal material by using the self-early-warning anti-corrosion paint and a self-early-warning anti-corrosion coating formed on the surface of the metal material by using the method. According to the invention, by utilizing the physical barrier effect of zirconium phosphate and the passivation, corrosion inhibition and color development effects of tannic acid, the corrosion self-early warning and long-acting protection of the coating on the metal material are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of multifunctional anti-corrosion coatings, and in particular to a self-warning anti-corrosion paint, an anti-corrosion coating and applications thereof in the anti-corrosion of metal materials. Background Art

[0002] Metal corrosion is an inevitable naturally occurring chemical process. The main purpose of metal protection methods is to prevent or reduce metal corrosion.

[0003] Among the many metal protection methods, anti-corrosion coating is one of the most effective means to reduce metal corrosion. Anti-corrosion coating is a special protective layer applied to the metal surface to prevent or reduce the harmful effects of corrosion. However, micropores and defects formed during the curing process of the coating will lead to its lack of long-term anti-corrosion performance.

[0004] In response to the problem that anti-corrosion coating materials lack long-term anti-corrosion performance, one method of metal protection is to introduce two-dimensional sheet materials into the anti-corrosion coating to utilize the two-dimensional sheet materials to construct a "maze effect" and improve the shielding performance of the anti-corrosion coating.

[0005] The patent application documents with publication numbers CN116285462A, CN118048061A, and CN116948497A reported so far all involve the application of carbon nanosheets, diamond nanosheets, and graphene two-dimensional sheet materials in anti-corrosion coatings. However, since the anti-corrosion coatings provided by the above-reported patent applications have a single function and expensive materials, they cannot solve the long-term anti-corrosion problem that is widely used in industrial production in different fields.

[0006] Another method to extend the anti-corrosion performance of the coating is to introduce a corrosion inhibitor into the coating matrix. The corrosion inhibitor can fill the pores in the coating caused by solvent evaporation during the preparation of the anti-corrosion coating, making the anti-corrosion coating denser; it can also repair the anti-corrosion coating when scratches appear, thereby improving the anti-corrosion performance of the coating.

[0007] Zirconium phosphate (α-ZrP) is a new type of multifunctional hierarchical material developed in recent years. Due to its high aspect ratio and morphologically controllable molecular structure, zirconium phosphate is often considered a model for studying two-dimensional lamellar materials and has been widely used in lubrication, corrosion resistance and other fields. Compared with traditional two-dimensional lamellar materials, zirconium phosphate exhibits better load-bearing capacity and wear resistance under higher loads. And because zirconium phosphate has excellent thermal stability, it can maintain the long-term corrosion resistance of the anti-corrosion coating at high temperatures.

[0008] In addition, tannic acid (TA) is introduced into the anti-corrosion coating as a corrosion inhibitor and corrosion warning agent (corrosion probe). When microcracks appear inside the anti-corrosion coating, they can be discovered and repaired in time at an early stage, which is conducive to realizing the corrosion self-warning function and long-term anti-corrosion performance of the anti-corrosion coating. However, if the corrosion inhibitor and corrosion warning agent are directly introduced into the coating, the reagent will be released prematurely in the anti-corrosion coating. In order to solve this problem, the corrosion inhibitor and / or corrosion warning agent are usually placed in a nanocontainer and then dispersed in the anti-corrosion coating matrix. In addition, the nanocontainer can effectively improve the compatibility of the anti-corrosion coating matrix with the corrosion inhibitor and / or corrosion warning agent, prolong the release time of the corrosion inhibitor, and realize the long-term protection function of the coating.

[0009] The effective combination of the barrier properties of two-dimensional sheet materials and the corrosion self-warning properties of corrosion inhibitors, and the optimization design of the coating structure, are of great research significance for realizing the corrosion self-warning function and long-term anti-corrosion performance of the coating. Summary of the invention

[0010] 1. Technical issues:

[0011] (1) The micropores and defects formed in the curing process of the existing anti-corrosion coating will cause the corrosion medium to penetrate, resulting in poor anti-corrosion performance of the anti-corrosion coating;

[0012] (2) The long-term anti-corrosion performance of existing anti-corrosion coatings is still unsatisfactory;

[0013] (3) The specific corrosion location inside the existing anti-corrosion coating cannot be determined during use;

[0014] (4) Lack of multifunctional coatings with corrosion warning and long-term corrosion protection.

[0015] (II) Technical solution:

[0016] In order to solve the above technical problems, the present invention provides a self-warning anti-corrosion coating in the first aspect, wherein the self-warning long-term anti-corrosion coating comprises a first coating and a second coating. The first coating comprises a modified zirconium phosphate and a first coating matrix; the second coating comprises silica microcapsules and a second coating matrix. The modified zirconium phosphate is prepared by modifying zirconium phosphate with a modifier; the silica microcapsules are prepared by impregnating mesoporous silica with tannic acid so that the silica microcapsules are loaded with tannic acid.

[0017] In a second aspect, the present invention provides a method for anti-corrosion treatment of metal materials, the method comprising the step of coating the metal material with the self-warning anti-corrosion coating described in the first aspect of the present invention.

[0018] The present invention provides a self-warning anti-corrosion coating in a third aspect. The self-warning anti-corrosion coating is formed on the surface of a metal material using the method described in the second aspect of the present invention.

[0019] Compared with the prior art, the present invention has the following technical advantages:

[0020] (1) The present invention fills the modified zirconium phosphate (a two-dimensional sheet material) and the silica microcapsules loaded with tannic acid into the resin matrix respectively and sprays them in layers. The upper zirconium phosphate coating uses the shielding properties of the sheet material to play a physical barrier role, so that the corrosive medium is effectively blocked at the initial stage of penetration. On the one hand, the silica microcapsules in the lower coating can fill the pores generated inside the resin during the curing process, making the coating more dense and making it difficult for the corrosive medium to penetrate; on the other hand, the tannic acid loaded by the silica microcapsules can react with metal materials such as steel plates to form a passivation film through a complex reaction, thereby playing a corrosion inhibition role. Since tannic acid can only form a passivation film after contacting the metal substrate, the silica microcapsules loaded with tannic acid are added to the bottom layer of the coating in the layered coating structure. The present invention utilizes the synergistic effect of zirconium phosphate and tannic acid in this way, which can effectively improve the long-term anti-corrosion performance of the coating. According to the test, the coating prepared by the present invention is immersed in salt water (for example, 3.5wt% NaCl aqueous solution, 25°C) for 100 days, and the impedance modulus (|Z| 0.01Hz ) can still maintain at 10 9 Ω·cm 2 Above, and most can be maintained at 10 10 Ω·cm 2 above.

[0021] (2) The present invention impregnates tannic acid into mesoporous silica (e.g., vacuum impregnation). During the process of corrosive solution penetrating the coating, tannic acid is released from the mesoporous silica and undergoes a complex reaction with the metal steel plate (color change may occur during the reaction process). At this time, tannic acid, as a corrosion inhibitor and corrosion probe, can sense the internal corrosion site of the coating through color change, so that the coating also has an anti-corrosion self-warning function.

[0022] (3) The layered self-warning long-term anti-corrosion coating prepared by the present invention can still maintain a high level of impedance modulus under high temperature and high salt conditions (90°C, 12wt% NaCl aqueous solution, 120 hours) and has excellent anti-corrosion performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A schematic diagram showing the layered structure of the self-warning anti-corrosion coating of the present invention.

[0024] Figure 2 The SEM image of the cross section of the self-warning anti-corrosion coating prepared in Example 4 of the present application is shown.

[0025] Figure 3 The scratch test results performed in Example 4 are shown, including optical photographs of the pure EP scratch coating immersed in 3.5wt% salt water on the 0th day (a1) and the 10th day (a2), and optical photographs of the composite coating of the layered structure of the present invention immersed in 3.5wt% salt water on the 0th day (b1) and the 10th day (b2).

[0026] The reference numerals are as follows: 1 represents modified zirconium phosphate; 2 represents silica microcapsules; 3 represents color development (purple-black) self-warning phenomenon; 4 represents metal material; 5 represents upper coating layer; and 6 represents lower coating layer. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In a first aspect, the present invention provides a self-warning anti-corrosion coating, the self-warning long-term anti-corrosion coating comprising a first coating and a second coating. The first coating comprises modified zirconium phosphate and a first coating matrix; the second coating comprises silica microcapsules and a second coating matrix. The modified zirconium phosphate is prepared by modifying zirconium phosphate with a modifier; the silica microcapsules are prepared by impregnating mesoporous silica with tannic acid so that the silica microcapsules are loaded with tannic acid.

[0029] Some coating substrates may require a curing agent (e.g., according to the recommendations of the instructions for commercially available coating substrates or sometimes require faster curing). In this case, the first coating and / or the second coating may contain a curing agent in an amount required for curing. However, those skilled in the art are fully capable of selecting a suitable curing agent and its amount after reading this application.

[0030] In some preferred embodiments, the modifier is selected from one of 3-(trimethoxysilyl)propyl methacrylate (sometimes referred to as KH550), 3-glycidoxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.

[0031] The first coating matrix and the second coating matrix may be the same or different.

[0032] Preferably, the first coating matrix and the second coating matrix are independently resin matrices. More preferably, the first coating matrix and the second coating matrix are independently selected from at least one of epoxy resin, polyurea resin and polyurethane.

[0033] In other preferred embodiments, the modified zirconium phosphate is prepared by the following method: (i) dispersing zirconium phosphate ((α-ZrP)) in a buffer solution to obtain a zirconium phosphate dispersion; (ii) dissolving a modifier in a modifying solvent to obtain a modifier solution; (iii) adding the zirconium phosphate dispersion to the modifier solution to carry out a modification reaction to obtain modified zirconium phosphate.

[0034] In other preferred embodiments, the buffer is a tris(hydroxymethyl)aminomethane aqueous buffer solution with a concentration of 0.01 M to 0.05 M (eg, 0.02, 0.03 or 0.04 M).

[0035] More preferably, the mass fraction of zirconium phosphate in the zirconium phosphate dispersion is 0.5% to 3% (eg, 1% or 2%).

[0036] In some other preferred embodiments, the dispersion is carried out by ultrasonic dispersion. Preferably, the ultrasonic dispersion time is 20 minutes to 40 minutes (eg, 30 minutes).

[0037] In some other preferred embodiments, after dispersion, the pH of the zirconium phosphate dispersion is adjusted (for example, using a 1 M HCl aqueous solution) to pH=1 to 3 (for example, pH=2).

[0038] In a more specific embodiment, the modified zirconium phosphate is prepared by the following method: preparing a tris (hydroxymethyl)aminomethane (Tris) aqueous buffer solution with a concentration of 0.01M to 0.05M, adding zirconium phosphate (α-ZrP) (the mass fraction of α-ZrP in the Tris buffer solution is 0.5% to 3%), ultrasonically dispersing for 20 minutes to 40 minutes, and then slowly adding 1M HCl to adjust the pH to 1 to 3 to obtain a zirconium phosphate-tris (hydroxymethyl)aminomethane mixed solution.

[0039] In other preferred embodiments, the modified solvent is ethanol.

[0040] More preferably, the mass fraction of the modifier in the modifier solution is 0.25% to 1.5% (eg, 0.5, 1.0 or 1.25%).

[0041] In other preferred embodiments, the dissolution of the modifier in the modifying solvent may be achieved by heating at 50-70° C. (eg, in a water bath) for 30 to 60 minutes.

[0042] In step (iii), the volume ratio of the zirconium phosphate dispersion to the modifier solution can be 1: 1. The addition method can be dropwise addition, and after addition, the mixture can be stirred for, for example, 5 to 10 hours (stirring speed 300-500 rpm), and then washed, filtered, and dried to obtain modified zirconium phosphate.

[0043] In a more specific embodiment, a modifier such as 3-(trimethoxysilyl)propyl methacrylate (KH550) can be dissolved in anhydrous ethanol (the mass fraction of KH550 is 0.25% to 1.5%), and heated in a water bath at 50-70° C. for 30 to 60 minutes to obtain a modifier solution. Then, the zirconium phosphate dispersion (such as a zirconium phosphate-trishydroxymethylaminomethane mixed solution) is added dropwise to the modifier solution (the volume ratio of the two solutions can be 1:1), stirred for 5 to 10 hours, washed, filtered, and dried to obtain zirconium phosphate modified by the modifier (such as KH550), that is, modified zirconium phosphate.

[0044] In other preferred embodiments, the particle size of the mesoporous silica is 100 nm to 2 μm (eg, 400 or 500 nm).

[0045] In other preferred embodiments, the mass ratio of tannic acid to mesoporous silica used in the impregnation is 1 to 3:1 (eg, 2:1).

[0046] In other preferred embodiments, the silica microcapsules are prepared by the following method: (I) dispersing the template in a template dispersion and emulsifying to obtain a template emulsion; (II) adding a silica precursor to the template emulsion for coating reaction to obtain silica-coated template microcapsules; (III) heating the silica-coated template microcapsules to obtain mesoporous silica; (IV) impregnating the mesoporous silica with tannic acid to obtain silica microcapsules loaded with tannic acid.

[0047] In other preferred embodiments, the template agent is hexadecyltrimethylammonium bromide.

[0048] In other preferred embodiments, the template dispersion is a mixed solution of ethanol and deionized water in a mass ratio of 9:1 to 1:4.

[0049] In some other preferred embodiments, the mass fraction of the template in the template emulsion is 0.3% to 2.0%.

[0050] In other preferred embodiments, the silicon dioxide precursor is tetraethyl orthosilicate.

[0051] In some other preferred embodiments, the heating temperature of the heat treatment is 400 to 800° C., and the treatment time is 3 to 5 hours.

[0052] In some more specific embodiments, the mesoporous silica can be prepared in the following manner: prepare a mixed solution of anhydrous ethanol and deionized water (the mass ratio of anhydrous ethanol to water can be 9:1 to 1:4), add 0.3% to 2.0% of hexadecyl trimethyl ammonium bromide (CTAB), and emulsify at high speed for 5 minutes (emulsification speed 5000 to 8000rpm) to obtain a template solution. The template solution is transferred to a three-necked flask, and 2% to 5% of ethyl orthosilicate is added, and the pH of the system is adjusted to 10 to 12 with, for example, ammonia water, and stirred in a water bath at 50-80°C for 2 to 6 hours (stirring speed 500-800rpm), washed, filtered, and dried to obtain silica microcapsules coated with the template. The silica-coated template microcapsules are heated at 400 to 800° C. (for example, a muffle furnace can be used) for 3 to 5 hours to obtain mesoporous silica (MSN) (particle size 100 nm to 2 μm).

[0053] During the impregnation, tannic acid and mesoporous silica can be mixed at a mass ratio of 1 to 3:1, and the mixture obtained is dispersed in anhydrous ethanol (the mass ratio of the mixture in anhydrous ethanol is 5%-20%), and moved into a vacuum drying oven (can be at 25°C under a vacuum degree of 0.06 to 0.09), taken out and stirred evenly after 20-60 minutes, and then put into the vacuum drying oven again, and repeated 2 to 3 times. After washing, filtering and drying the obtained suspension, silica microcapsules loaded with tannic acid (sometimes referred to as TA@MSN herein) are obtained.

[0054] If necessary, the anticorrosive coating may contain an optional curing agent. The present invention has no particular limitation on the curing agent, and the type and amount thereof may be selected within the capabilities of those skilled in the art.

[0055] The second aspect of the present invention is a method for anti-corrosion treatment of metal materials, which includes the step of coating the metal material with the self-warning anti-corrosion coating described in the first aspect of the present invention.

[0056] In some preferred embodiments, the coating process is carried out in two steps: (a) coating the second coating on the metal material to form a base coating; (b) coating the first coating on the base coating to form an upper coating, and then curing the coating.

[0057] In some embodiments, in the second coating, the amount of the silica microcapsules relative to the first coating substrate (if a curing agent is used, relative to the total mass of the first coating substrate and the curing agent) is 2 mass% to 20 mass% (for example, 5, 10 or 15 mass%), preferably 5 mass% to 15 mass%. After the silica microcapsules are added to the coating substrate and stirred evenly, they can be sprayed onto the surface of the metal material (for example, a steel plate) at a spraying pressure of 0.6MPa to 1.0MPa (for example, 0.7, 0.8 or 0.9MPa) at room temperature to 130°C (for example, 30, 40, 50, 60, 70, 80, 90, 100, 110 or 120°C) to form a base coating. Preferably, the thickness of the base coating can be 30μm to 100μm, for example, 50, 60, 70, 80 or 90μm.

[0058] After forming the bottom coating, the top coating is then formed on the bottom coating. In some embodiments, in the first coating, the amount of the modified zirconium phosphate relative to the second coating substrate (if a curing agent is used, relative to the total mass of the second coating substrate and the curing agent) is 5 mass % to 40 mass % (for example, 10, 20 or 30 mass %), preferably 10 mass % to 30 mass %, and more preferably 10 mass % to 20 mass %. After the modified zirconium phosphate is stirred evenly in the coating substrate, it can be sprayed onto the surface of the bottom coating at a temperature of room temperature to 130°C (for example, 30, 40, 50, 60, 70, 80, 90, 100, 110 or 120°C) and a spraying pressure of 0.6MPa to 1.0MPa (for example, 0.7, 0.8 or 0.9MPa) to form a top coating. Preferably, the thickness of the upper coating layer may be 60 μm to 200 μm, for example, 80, 100, 120, 140, 160 or 180 μm.

[0059] Therefore, the total thickness of the anti-corrosion coating prepared by the method of the present invention may be 100 μm to 300 μm, for example 200 μm.

[0060] For the convenience of coating, some types of epoxy resins as coating substrates need to be appropriately diluted with diluents (such as ethyl acetate) for convenient spraying, while some coating substrates such as water-based polyurethanes do not need to be diluted with diluents. The specific dilution degree is entirely within the ability of those skilled in the art after reading this specification.

[0061] In some preferred embodiments, the curing of the bottom coating and the curing of the upper coating can be independently cured at room temperature for 12 hours to 4 hours (e.g., 15, 18 or 21 hours), and then cured at 40°C to 100°C (e.g., 50 or 80°C) for 3 hours to 6 hours (4 or 5 hours). Finally, a layered self-warning long-term anti-corrosion coating with a coating thickness of 100-300 μm is obtained.

[0062] The metal material may be an iron material (such as a steel pipe material or a steel plate material or other profiles), an aluminum material or a copper material, etc. When the metal material is a steel plate material, the model of the steel plate material may be one of the models of steel plates such as Q195, Q235, and Q345.

[0063] Before coating, the metal material, such as the steel plate material, can be ground, polished and rinsed. The grinding can be performed using sandpaper. The selected sandpaper can be 600 mesh, 800 mesh or 1000 mesh sandpaper. The solvent used for rinsing can be at least one of ethanol, acetone or ethyl acetate.

[0064] In some embodiments, the coating is performed by spraying. For example, the spraying can be performed while maintaining the temperature of the metal material at 80° C. to 130° C. (eg, 90, 100, 110, or 120° C.), and the spraying pressure can be 0.6 MPa to 1.0 MPa.

[0065] The present invention provides a self-warning anti-corrosion coating in a third aspect. The self-warning anti-corrosion coating is formed on the surface of a metal material using the method described in the second aspect of the present invention.

[0066] Figure 1 A schematic diagram showing the layered structure of the self-warning anti-corrosion coating of the present invention is shown. Figure 1 As shown, the anti-corrosion behavior of the upper zirconium phosphate layer is mainly reflected in the initial stage of immersion, and the physical shielding effect is used to effectively prevent the penetration of corrosive media; in addition, if the corrosive medium penetrates the zirconium phosphate layer during long-term immersion, the anti-corrosion behavior of the coating is mainly reflected by the underlying silica microcapsule layer. Tannic acid, as a corrosion inhibitor and corrosion probe, is released from the silica microcapsules during the immersion process and adsorbed onto the surface of the metal steel plate to form an adsorption layer (passivation film), which can further prevent the penetration of corrosive media and play an anti-corrosion role on the one hand; on the other hand, the color of the adsorption layer changes during the formation process, from light yellow to purple-black, which can provide early warning of the corrosion condition inside the coating, accurately determine the corrosion site, and carry out repairs. The present invention prepares a long-lasting anti-corrosion coating with a simple process and the dual functions of self-warning and self-repair.

[0067] The filler composition of the present invention can be used to form a layered structure of an anticorrosive coating on a metal material, using the physical shielding effect of the zirconium phosphate layer to achieve early anticorrosion, while using the later repair effect of the underlying silica microcapsule layer to achieve synergistic anticorrosion, so that the coating has long-term anticorrosion performance. In addition, the coating of the present invention can accurately determine the internal corrosion site of the coating through color changes, so that it can be repaired in time.

[0068] Example

[0069] Preparation Example 1: Preparation of modified zirconium phosphate

[0070] This step provides for modifying zirconium phosphate using a modifier, and the specific method is as follows:

[0071] Prepare 100 mL of tris (hydroxymethylaminomethane) (Tris) aqueous buffer solution with a concentration of 0.02 M, add 1 g of zirconium phosphate (α-ZrP), ultrasonically disperse for 20 minutes, and then add 1 M HCl to adjust the pH to 2 to obtain a zirconium phosphate-tris (hydroxymethylaminomethane) mixed solution.

[0072] 0.5 g of 3-(trimethoxysilyl)propyl methacrylate (KH550) was dissolved in 100 mL of anhydrous ethanol. After heating in a water bath at 60°C for 30 minutes, a zirconium phosphate-trishydroxymethylaminomethane mixed solution was added dropwise to the solution and stirred for 8 hours. After washing, filtration and drying, KH550-modified zirconium phosphate (modified ZrP) was obtained.

[0073] Preparation Example 2: Preparation of Silica Microcapsules

[0074] First, a one-step method is used to prepare silica coated with a template, and the coated template is removed at high temperature in a muffle furnace to obtain mesoporous silica. Specifically, a mixed solution of anhydrous ethanol and distilled water with a mass ratio of 1:2 (80 ml of anhydrous ethanol and 160 ml of distilled water) is prepared, 0.8 g of hexadecyltrimethylammonium bromide (CTAB) is added, and then high-speed emulsification is performed for 5 minutes (emulsification speed 5000 rpm), and then transferred to a three-necked flask, and 3 mL of tetraethyl orthosilicate is added, and the pH is adjusted to 10 with ammonia water, and stirred in a water bath at 80°C for 3 hours (stirring speed 800 rpm), washed, filtered, and dried to obtain silica coated with a template. Finally, the silica coated with a template is heated in a muffle furnace at 600°C for 5 hours to obtain mesoporous silica (MSN) (particle size 450 nm).

[0075] The prepared mesoporous silica (MSN) was vacuum impregnated with tannic acid to obtain silica microcapsules (TA@MSN) loaded with tannic acid. Specifically, a mixture of tannic acid and mesoporous silica with a mass ratio of 2:1 (tannic acid 0.2g, mesoporous silica 0.1g) was dissolved in 10ml of anhydrous ethanol and moved into a vacuum drying oven (25°C, vacuum degree 0.09). After 40 minutes, it was taken out and stirred evenly, and then put into the vacuum drying oven again, and repeated 3 times. After washing, filtering and drying the obtained suspension, silica microcapsules (TA@MSN) containing tannic acid were obtained.

[0076] Example 1: Preparation of anti-corrosion coating for metal materials

[0077] In this embodiment, a steel plate is used as the metal material, and a layered structure including a bottom coating and an upper coating is sequentially formed on the surface as an anti-corrosion coating.

[0078] (A) Preparation of metal materials

[0079] The steel plate is ground, polished, and repeatedly rinsed with water and solvent. Specifically, the Q235 steel plate is ground with 600-mesh and 1000-mesh sandpapers in sequence, and rinsed with water and anhydrous ethanol in sequence to remove surface stains, thereby obtaining a steel plate to be coated.

[0080] (B) Preparation of base coating

[0081] The silica microcapsules loaded with tannic acid are added into the coating matrix to prepare the second coating, which is then sprayed onto the surface of the steel plate to prepare the base coating.

[0082] Specifically, in order to conduct a comparative study, the inventors first prepared a pure resin coating without any filler. 2.4g E51 epoxy resin and 0.8g D230 curing agent were dissolved in 10ml ethyl acetate, stirred to prepare a pure EP homogeneous solution, and sprayed on the surface of Q235 steel plate at a temperature of 100°C and a spraying pressure of 0.6MPa. After curing at room temperature for 12 hours, it was cured at 60°C for 3h to obtain a pure EP coating with a thickness of 120μm.

[0083] 0.9 g E51 epoxy resin and 0.3 g D230 curing agent were dissolved in 10 ml ethyl acetate, and 0.12 g TA@MSN was added and stirred evenly to obtain a second coating; the second coating was sprayed onto the surface of a Q235 steel plate at a temperature of 100°C and a spraying pressure of 0.6 MPa to prepare a silica microcapsule coating as a base coating with a thickness of 40 μm.

[0084] (C) Preparation of upper coating

[0085] The modified zirconium phosphate is filled into the first coating matrix to prepare a first coating, and then sprayed onto the surface of the aforementioned bottom coating to prepare an upper coating.

[0086] Specifically, 1.5 g of E51 epoxy resin and 0.5 g of D230 curing agent were dissolved in 10 ml of ethyl acetate, and 0.40 g of modified zirconium phosphate was added and stirred to obtain the first coating, which was then sprayed onto the surface of the silica microcapsule coating (i.e., the bottom coating) at a temperature of 100° C. and a spraying pressure of 0.6 MPa to prepare a zirconium phosphate coating (i.e., the upper coating) with a thickness of 80 μm.

[0087] At this point, a layered structure including a bottom coating and an upper coating is formed on the steel plate (see Figure 2 ).

[0088] (D) Curing of coating

[0089] The prepared composite coating is cured to obtain a composite coating with a layered structure.

[0090] Specifically, the sprayed composite coating was cured at room temperature for 12 hours and then cured at 60°C for 3 hours to finally obtain a self-warning long-acting layered anti-corrosion coating with a coating thickness of 120 μm.

[0091] After testing, it was found that the layered self-warning long-term anti-corrosion coating prepared in this embodiment can detect and warn of metal corrosion in a timely manner.

[0092] First, the anticorrosion coating prepared in this example was immersed in a 3.5wt% NaCl solution for 100 days, |Z| 0.01Hz Still maintained at 10 10 Ω·cm 2 Above; after immersion for 120 hours under extreme conditions of high temperature and high salt (90°C, 12wt% NaCl aqueous solution), |Z| 0.01Hz It can still reach 8.05×10 9 Ω·cm 2 .

[0093] Secondly, the prepared layered coating was scratched, and the scratches were deep enough to reach the base of the steel plate to ensure that the steel plate was exposed to the corrosive environment. At the same time, for comparative research, the pure epoxy coating was also scratched. After the two scratched coatings were immersed in a 3.5wt% NaCl aqueous solution at room temperature for 10 days, the pure EP coating surface showed blistering and more serious corrosion; while the layered coating of the present invention had a dense surface and good repair performance, and a purple-black self-warning phenomenon appeared at the scratch (see Figure 3 This is mainly due to the redox reaction on the metal surface producing abundant Fe 3+When it encounters tannic acid released from mesoporous silica, it generates purple-black tannic acid-Fe 3+ The layered coating prepared in Example 1 exhibits excellent self-warning and long-term anti-corrosion performance.

[0094] Examples 2 to 12

[0095] Except for the contents shown in Table 1 below, the same method as in Example 1 was followed.

[0096] Table 1. The content of modified zirconium phosphate in the first coating and the content of silica microcapsules in the second coating used in each example and the anticorrosion performance of the formed coating

[0097]

[0098] Note: Modified ZrP is the modified zirconium phosphate prepared in Preparation Example 1; TA@MSN is the silica microcapsule prepared in Preparation Example 2; the content represents the mass percentage (mass %) of the modified zirconium phosphate or silica microcapsule relative to the coating matrix and curing agent (if used) in the corresponding coating.

[0099] |Z| 0.01Hz The value can be used as an indicator to evaluate the anti-corrosion performance of the coating. During the entire immersion process, the |Z| 0.01Hz Under normal conditions and high temperature and high salt conditions, the |Z| 0.01Hz It remains at the highest level under both normal conditions and high temperature and high salt conditions. It is worth noting that the layered composite coating has a new function of self-warning while having high impedance (good anti-corrosion effect and no blistering).

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A self-warning anti-corrosion coating, characterized in that: The self-warning long-term anti-corrosion coating comprises a first coating and a second coating, wherein the first coating comprises modified zirconium phosphate and a first coating matrix; and the second coating comprises silicon dioxide microcapsules and a second coating matrix; The modified zirconium phosphate is prepared by modifying zirconium phosphate using a modifier; The silica microcapsules are prepared by impregnating mesoporous silica with tannic acid so that the tannic acid is loaded inside the silica microcapsules.

2. The self-warning anti-corrosion coating according to claim 1 is characterized in that: The modifier is selected from one of 3-(trimethoxysilyl)propyl methacrylate, 3-glycidyloxypropyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane.

3. The self-warning anti-corrosion coating according to claim 1 is characterized in that: The first coating matrix and the second coating matrix are independently resin matrices; Preferably, the first coating matrix and the second coating matrix are independently selected from at least one of epoxy resin, polyurea resin and polyurethane; More preferably, in the first coating, the amount of the modified zirconium phosphate relative to the first coating substrate is 5% to 40% by mass, preferably 10% to 30% by mass, and more preferably 10% to 20% by mass; and / or in the second coating, the amount of the silica microcapsules relative to the second coating substrate is 2% to 20% by mass, preferably 5% to 15% by mass.

4. The self-warning anti-corrosion coating according to claim 3 is characterized in that: The modified zirconium phosphate is prepared by the following method: (i) dispersing zirconium phosphate in a buffer solution to obtain a zirconium phosphate dispersion; (ii) dissolving the modifier in a modifying solvent to obtain a modifier solution; (iii) adding the zirconium phosphate dispersion into the modifier solution to carry out a modification reaction to obtain modified zirconium phosphate.

5. The self-warning anti-corrosion coating according to claim 4 is characterized in that: The buffer solution is a tris(hydroxymethyl)aminomethane aqueous buffer solution with a concentration of 0.01M to 0.05M; preferably, the mass fraction of zirconium phosphate in the zirconium phosphate dispersion is 0.5% to 3%; and / or The modification solvent is one of ethanol and water; preferably, the mass fraction of the modifier in the modifier solution is 0.25% to 1.5%.

6. The self-warning anti-corrosion coating according to any one of claims 1 to 5, characterized in that: The particle size of the mesoporous silica is 100 nm to 2 μm; Preferably, the mass ratio of tannic acid to mesoporous silica used in the impregnation is 1 to 3:

1.

7. The self-warning anti-corrosion coating according to claim 6 is characterized in that: The silicon dioxide microcapsules are prepared by the following method: (I) dispersing the template in a template dispersion and emulsifying to obtain a template emulsion; (II) adding a silica precursor to the template emulsion to carry out a coating reaction to obtain silica-coated template microcapsules; (III) heating the silica-coated template microcapsules to obtain mesoporous silica; (IV) impregnating the mesoporous silica with tannic acid to obtain silica microcapsules loaded with tannic acid; Preferably, the template agent is hexadecyltrimethylammonium bromide; The template dispersion is a mixed solution of ethanol and deionized water in a mass ratio of 9:1 to 1:4; Preferably, the mass fraction of the template in the template emulsion is 0.3% to 2.0%; Preferably, the silicon dioxide precursor is tetraethyl orthosilicate; The heating temperature of the heat treatment is 400 to 800° C., and the treatment time is 3 to 5 hours.

8. A method for anti-corrosion treatment of metal materials, characterized in that: The method comprises the step of coating a metal material with the self-warning anti-corrosion coating according to any one of claims 1 to 7.

9. The method according to claim 8, characterized in that The method comprises the following steps: (a) applying the second coating on the surface of the metal material to form a base coating; (b) applying the first coating material on the base coating to form an upper coating layer, and then curing the coating layer.

10. A self-warning anti-corrosion coating, characterized in that: The self-warning anti-corrosion coating is formed on the surface of the metal material by the method described in claim 9; Preferably, the thickness of the bottom coating layer may be 30 μm to 100 μm; and / or the thickness of the top coating layer may be 60 μm to 200 μm.

Citation Information

Patent Citations

  • Anticorrosive coating having self repair capability, and preparation method and application of anticorrosive coating

    CN107502133A

  • Dual self-repairing anticorrosive coating and preparation method thereof

    CN115433478A

  • Intelligent coating with double functions of corrosion repair and early-stage corrosion early warning as well as preparation method and application of intelligent coating

    CN116948506A

  • Anti-corrosive coating with self-repairing ability, preparation method therefor, and application thereof

    WO2019029172A1

Cited By

  • Bionic patterned biomass-based photoluminescence polyurethane coating for leather and preparation method of bionic patterned biomass-based photoluminescence polyurethane coating