Bonding blocking agent for high-viscosity and high-elasticity modified asphalt and preparation process of bonding blocking agent

By using a bonding inhibitor containing a specific compound on the construction equipment, the adhesion problem between the high-viscosity and high-elasticity modified asphalt and the construction equipment was solved, enabling smooth flow and uniform paving of the asphalt mixture, and improving the compaction effect and service life of the road surface.

CN118931376AActive Publication Date: 2024-11-12GUANGDONG LONGSHENGDA NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410992323.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

High-viscosity and high-elasticity modified asphalt materials are prone to sticking to construction equipment during construction, causing construction problems. Existing anti-adhesion materials are not very effective, especially for high-viscosity and high-elasticity modified asphalt.

Method used

Adhesion blocking agents containing compounds such as AdBlock-01, cis-3-hexenyl hexanoate, trans-2-hexenyl hexanoate, or cis-3-hexenyl hexenoate are applied to the construction equipment by spraying or brushing to prevent the adhesion between the high-viscosity, high-elasticity modified asphalt and the equipment.

Benefits of technology

It effectively prevents the adhesion of high-viscosity and high-elasticity modified asphalt to transport vehicles, pavers, road rollers and other equipment, ensuring the smooth flow and uniform paving of asphalt mixture, improving the compaction effect of road rollers, and enhancing the smoothness and density of the road surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959195860000021
    Figure BDA0004959195860000021
  • Figure BDA0004959195860000031
    Figure BDA0004959195860000031
  • Figure BDA0004959195860000061
    Figure BDA0004959195860000061
Patent Text Reader

Abstract

In order to solve the problem of adhesion between high-viscosity and high-elasticity modified asphalt materials widely applied to asphalt pavement maintenance or construction markets and construction equipment, the invention provides the adhesion blocking agent between the high-viscosity and high-elasticity modified asphalt and the production equipment, and the adhesion blocking agent can efficiently block the adhesion between the high-viscosity and high-elasticity modified asphalt and the construction equipment. The application of the high-viscosity and high-elasticity modified asphalt and the construction of asphalt pavements are convenient. When a high-viscosity and high-elasticity modified asphalt mixture is produced, the bonding blocking agent is sprayed or brushed at the bottom and the periphery of a transport carriage and the periphery of a receiving hopper of a paver in advance. In some embodiments of the present invention, the adhesion blocker comprises the compound AdBlock-01.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of traffic construction, and in particular to a bonding blocker for high-viscosity and high-elasticity modified asphalt. Background Art

[0002] Hot mix asphalt mixture is widely used in highway construction and municipal road construction (Technical Specifications for Highway Asphalt Pavement Construction (JTGF40-2004)). Since the asphalt material in it is in liquid state under high temperature and has a certain bonding strength, during the production and application process, it is easy to contact with the transport vehicle compartment, paver hopper, steel wheel of steel wheel roller and tire of rubber wheel roller, which may cause adhesion and be difficult to remove. At present, the commonly used anti-adhesion materials include kerosene, vegetable oil, glycerin, etc. Kerosene has certain toxicity and damages the performance of asphalt mixture and is prohibited from use. Vegetable oil and glycerin also have a significant adverse effect on the performance of asphalt mixture, and the effect of preventing the adhesion between asphalt and construction equipment is poor, especially for the high-viscosity and high-elasticity modified asphalt commonly used in current road maintenance projects (Technical Guide for High-Toughness Ultra-Thin Asphalt Wear Layer (T / CHTS10130-2024)). The anti-adhesion effect is even more unsatisfactory. Therefore, the adhesion problem between high-viscosity and high-elasticity modified asphalt materials and construction equipment has caused great trouble to asphalt pavement construction. Summary of the invention

[0003] In order to solve the adhesion problem between high-viscosity and high-elasticity modified asphalt materials widely used in the asphalt pavement maintenance or construction market and construction equipment, a bonding blocker between high-viscosity and high-elasticity modified asphalt and production equipment is provided. By pre-coating the bonding blocker on the construction equipment that comes into contact with asphalt mixtures such as hot mix asphalt mixtures, the adhesion problem between the high-viscosity and high-elasticity modified asphalt and the construction equipment can be completely blocked, thereby facilitating the application of high-viscosity and high-elasticity modified asphalt and asphalt pavement construction.

[0004] The adhesion blocking agent described in the present invention is in liquid form. When the high-viscosity and high-elasticity modified asphalt mixture is produced, it is pre-sprayed or brushed on the bottom and around the transport vehicle box and around the receiving hopper of the paver to block the adhesion between the high-viscosity and high-elasticity modified asphalt and the transport vehicle box and the receiving hopper of the paver during the transportation of the high-viscosity and high-elasticity modified asphalt mixture by the transport vehicle and the paving process of the paver; when the roller is rolling the high-viscosity and high-elasticity modified asphalt mixture, it is intermittently sprayed on the steel wheel by the automatic spraying device of the steel wheel roller itself or is manually and frequently brushed on the tire of the rubber wheel roller to block the adhesion between the high-viscosity and high-elasticity modified asphalt and the steel wheel or rubber wheel of the roller during the rolling of the high-viscosity and high-elasticity modified asphalt mixture, thereby improving the rolling effect of the roller on the mixture.

[0005] In a first aspect of the present invention, a high-viscosity and high-elasticity modified asphalt adhesion blocker is provided, characterized in that the adhesion blocker comprises compound AdBlock-01, cis-3-hexenyl hexanoate, trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, and the structure of the compound AdBlock-01 is:

[0006]

[0007] In some embodiments of the invention, the adhesion blocking agent comprises the compound AdBlock-01 or cis-3-hexenoic acid cis-3-hexenyl ester.

[0008] In some embodiments of the present invention, the bonding blocker comprises cis-3-hexenyl hexanoate, trans-2-hexenyl hexanoate or cis-3-hexenyl hexenoate. In some embodiments of the present invention, the bonding blocker comprises cis-3-hexenyl hexanoate. In some embodiments of the present invention, the bonding blocker comprises trans-2-hexenyl hexanoate. In some embodiments of the present invention, the bonding blocker comprises cis-3-hexenyl hexanoate.

[0009] In some embodiments of the present invention, the adhesion blocking agent comprises the following ingredients by weight: 1% to 12% dimethicone, 1% to 14% glycerol, 30% to 60% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% sodium dodecylbenzene sulfonate, 1% to 5% alkylphenol polyoxyethylene ether, preservative, and the balance is water. In some embodiments of the present invention, the alkylphenol polyoxyethylene ether is octylphenol polyoxyethylene ether OP-10.

[0010] In some embodiments of the present invention, the adhesion blocking agent comprises the following ingredients by weight: 5% to 7% dimethicone, 10% to 14% glycerol, 30% to 50% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% sodium dodecylbenzene sulfonate, 1% to 5% alkylphenol polyoxyethylene ether OP-10, a preservative, and the balance is water.

[0011] In some embodiments of the present invention, the adhesion blocking agent comprises the following ingredients by weight: 1% to 12% dimethicone, 1% to 14% glycerol, 30% to 60% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% sodium dodecylbenzene sulfonate, 1% to 5% alkylphenol polyoxyethylene ether, 0.5% to 2% sodium benzoate, 0.5% to 2% flavor, and the balance is water.

[0012] In some embodiments of the present invention, the adhesion blocking agent comprises the following ingredients by weight: 6% dimethicone, 12% glycerol, 40% AdBlock-01 compound, 3% sodium dodecylbenzene sulfonate, and 3% alkylphenol polyoxyethylene ether OP-10.

[0013] In some embodiments of the present invention, the preparation method of the bonding blocker is as follows: the main ingredients are mixed, sheared at a speed of 4000r / min for 10 minutes using a shearing instrument, and then placed in an oven at 65°C for 30 minutes, sheared for another 10 minutes, and then placed in an oven at 65°C for another 30 minutes; preservatives and flavors are added, and then sheared for another 10 minutes, and then placed in an oven at 65°C for another 30 minutes; a high-viscosity and high-elasticity modified asphalt bonding blocker is obtained;

[0014] Optionally, the main component comprises the following ingredients by weight: 1% to 12% dimethicone, 1% to 14% glycerol, 30% to 60% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% sodium dodecylbenzene sulfonate, 1% to 5% alkylphenol polyoxyethylene ether OP-10, and an appropriate amount of water.

[0015] In some embodiments of the present invention, the preparation method of the adhesion blocking agent is as follows: 6 g of dimethyl silicone oil, 12 g of glycerol, compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate are mixed and heated to 65°C, stirred for 15 minutes, and then 3 g of sodium dodecylbenzene sulfonate, 3 g of octylphenol polyoxyethylene ether OP-10 and 36 g of water are added, and stirring is continued for 15 minutes; after shearing with a shearing instrument at a speed of 4000 r / min for 10 minutes, it is allowed to stand in an oven at 65°C for 30 minutes, sheared for another 10 minutes, and continued to stand in an oven at 65°C for 30 minutes; 1 g of sodium benzoate and 0.5 g of essence are added, and then sheared for another 10 minutes, and allowed to stand to room temperature.

[0016] The structure of the compound AdBlock-01 is:

[0017]

[0018] The two carbon-carbon double bonds of compound AdBlock-01 are both in trans configuration.

[0019] In some embodiments of the present invention, the preparation method of the adhesion blocking agent is as described in Example 2.

[0020] In some embodiments of the present invention, the adhesion blocking agent blocks or reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the carriage of the transport vehicle, the adhesion between the high-viscosity and high-elasticity modified asphalt and the receiving hopper of the paver, or the adhesion between the high-viscosity and high-elasticity modified asphalt and the steel wheel of the roller.

[0021] In some embodiments of the present invention, the adhesion blocking agent blocks the adhesion between the high-viscosity and high-elasticity modified asphalt and the carriage of the transport vehicle, blocks the adhesion between the high-viscosity and high-elasticity modified asphalt and the receiving hopper of the paver, or blocks the adhesion between the high-viscosity and high-elasticity modified asphalt and the steel wheel of the roller.

[0022] In some embodiments of the present invention, the adhesion blocking agent reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the carriage of the transport vehicle, reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the receiving hopper of the paver, or reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the steel wheel of the roller.

[0023] In some embodiments of the present invention, the adhesion blocking agent blocks or reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the carriage of the transport vehicle.

[0024] In some embodiments of the present invention, the adhesion blocking agent blocks or reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the receiving hopper of the paver.

[0025] In some embodiments of the present invention, the adhesion blocking agent blocks or reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the steel wheel of the roller.

[0026] In some embodiments of the present invention, the adhesion blocking agent blocks or reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the carriage of the transport vehicle during the transportation of the high-viscosity and high-elasticity modified asphalt mixture.

[0027] In some embodiments of the present invention, the adhesion blocking agent blocks or reduces the adhesion between the high-viscosity and high-elasticity modified asphalt and the steel wheel of the roller during the process of rolling the high-viscosity and high-elasticity modified asphalt mixture.

[0028] In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture comprises high-viscosity and high-elasticity modified asphalt, coarse aggregate, fine aggregate, and mineral powder. In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture comprises high-viscosity and high-elasticity modified asphalt, coarse aggregate, fine aggregate, and mineral powder.

[0029] In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture is an asphalt concrete mixture.

[0030] In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture is an asphalt macadam mixture.

[0031] In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture is a hot-mix asphalt mixture or a room-temperature asphalt mixture.

[0032] In the second aspect of the present invention, a method for preparing a high-viscosity and high-elasticity modified asphalt bonding blocker is provided, characterized in that the preparation method is: mixing the main components, shearing with a shearing instrument at a speed of 4000r / min for 10 minutes, standing in an oven at 65°C for 30 minutes, shearing for another 10 minutes, and continuing to stand in an oven at 65°C for 30 minutes; adding preservatives and flavors, shearing for another 10 minutes, and standing to room temperature to obtain a high-viscosity and high-elasticity modified asphalt bonding blocker;

[0033] The main components include the following components by weight: 1% to 12% of dimethyl silicone oil, 1% to 14% of glycerol, 30% to 60% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% of sodium dodecylbenzene sulfonate, alkylphenol polyoxyethylene ether, and an appropriate amount of water.

[0034] In some embodiments of the present invention, the main components include the following ingredients by weight: 1% to 12% dimethicone, 1% to 14% glycerol, 30% to 60% compound AdBlock-01 or cis-3-hexenoic acid cis-3-hexenyl ester, 1% to 5% sodium dodecylbenzene sulfonate, alkylphenol polyoxyethylene ether, and an appropriate amount of water.

[0035] In some embodiments of the present invention, the preparation method is used to prepare the adhesion blocking agent as described in the first aspect of the present invention.

[0036] In some embodiments of the present invention, the alkylphenol polyoxyethylene ether is octylphenol polyoxyethylene ether OP-10.

[0037] In some embodiments of the present invention, the main components include the following ingredients by weight: 5% to 7% dimethicone, 10% to 14% glycerol, 30% to 50% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% sodium dodecylbenzene sulfonate, 1% to 5% alkylphenol polyoxyethylene ether, and an appropriate amount of water.

[0038] In some embodiments of the present invention, the preparation method of the adhesion blocking agent is as follows: 6 g of dimethyl silicone oil, 12 g of glycerol, compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate are mixed and heated to 65°C, stirred for 15 minutes, and then 3 g of sodium dodecylbenzene sulfonate, 3 g of octylphenol polyoxyethylene ether OP-10 and 36 g of water are added, and stirring is continued for 15 minutes; after shearing with a shearing instrument at a speed of 4000 r / min for 10 minutes, it is allowed to stand in an oven at 65°C for 30 minutes, sheared for another 10 minutes, and continued to stand in an oven at 65°C for 30 minutes; 1 g of sodium benzoate and 0.5 g of essence are added, and then sheared for another 10 minutes, and allowed to stand to room temperature.

[0039] In the third aspect of the present invention, there is provided the use of the adhesion blocking agent as described in the first aspect in the transportation, paving and / or rolling of a highly viscous and highly elastic modified asphalt mixture.

[0040] In some embodiments of the present invention, there is provided use of the adhesion blocking agent as described in the first aspect in transporting high-viscosity and high-elasticity modified asphalt mixture.

[0041] In some embodiments of the present invention, there is provided use of the adhesion blocking agent as described in the first aspect in paving a high-viscosity and high-elasticity modified asphalt mixture.

[0042] In some embodiments of the present invention, there is provided use of the adhesion blocking agent as described in the first aspect in rolling a high-viscosity and high-elasticity modified asphalt mixture.

[0043] In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture comprises high-viscosity and high-elasticity modified asphalt, coarse aggregate, fine aggregate, and mineral powder. In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture comprises high-viscosity and high-elasticity modified asphalt, coarse aggregate, fine aggregate, and mineral powder.

[0044] In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture is an asphalt concrete mixture.

[0045] In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture is an asphalt macadam mixture.

[0046] In some embodiments of the present invention, the high-viscosity and high-elasticity modified asphalt mixture is a hot-mix asphalt mixture or a room-temperature asphalt mixture.

[0047] In a fourth aspect of the present invention, a compound is provided, the structure of the compound being:

[0048]

[0049] The two carbon-carbon double bonds of the compound are both in trans configuration.

[0050] The technical effects of the technical solution of the present invention are as follows:

[0051] After the adhesion blocker of the present invention is adopted, when the dump truck is unloading the high-viscosity and high-elastic modified asphalt mixture, as the front end of the carriage is lifted, the mixture in the carriage will flow smoothly from bottom to top into the receiving hopper of the paver, avoiding the blocking of the outflow of the mixture due to the adhesion between the high-viscosity and high-elastic modified asphalt and the vehicle body, and even when the carriage is lifted too high due to poor circulation, the mixture in the carriage suddenly falls due to gravity, causing the serious consequence of burying the paver or overturning the transport vehicle. After the adhesion blocker is brushed in the receiving hopper of the paver, sprayed on the steel wheel of the steel wheel roller, and sprayed or brushed on the tire of the rubber wheel roller, it can ensure that the asphalt mixture in the receiving hopper of the paver is uniform and less segregated, improve the uniformity of the paved asphalt mixture, ensure that the roller does not stick to the wheel when rolling the mixture under the high temperature state, and can effectively improve the compaction effect of the road surface, improve the flatness and density of the road surface, thereby improving the driving comfort and service life of the road surface. DETAILED DESCRIPTION

[0052] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications. Unless otherwise specified, the reagents and raw materials used in the present invention are all commercially available.

[0053] Example

[0054] Example 1: Synthesis and characterization of AdBlock-01, a key component of a high-viscosity and high-elasticity modified asphalt bonding blocker

[0055]

[0056] Take 100g of 5-decenoic acid (alfa-chemistry, Catalog No. ACM85392036) and dissolve it in 6L of n-propyl acetate, then add 100g of (E)-dec-3-en-1-ol (alfa-chemistry, Catalog No. ACM10339603). Slowly add 20mL of concentrated sulfuric acid. Reflux reaction for 7h, cool to room temperature. Extract with dilute sodium bicarbonate solution, take the organic phase, remove the solvent by vacuum rotary evaporation, and purify by silica gel column chromatography (petroleum ether / ethyl acetate 100:1) to obtain compound AdBlock-01, chemical name (E)-dec-3-en-1-yl(E)-dec-5-enoate, a colorless oil, purity 99.1%, yield 23%.

[0057] The NMR data of compound AdBlock-01 are as follows:

[0058] 1 H NMR(400MHz,DMSO-d6)δ5.76–5.39(m,2H),4.26(td,2H),2.73–2.58(m,4H ),2.43–2.24(m,6H),1.84(tt,2H),1.53–1.17(m,14H),1.02–0.75(m,6H).

[0059] 13 C NMR(100MHz,DMSO-d6)δ175.4,132.4,130.1,129.9,127.0,65.6,41.3,39 .2,38.9,38.1,36.4,34.7,31.3,28.1,27.5,25.8,23.9,21.0,14.5,13.1.

[0060] Example 2: Preparation of high-viscosity and high-elasticity modified asphalt bonding blocker

[0061] 6 g of dimethyl silicone oil, 12 g of glycerol, and 40 g of the AdBlock-01 compound prepared as described in Example 1 were added to a round-bottom flask in sequence, mixed, heated to 65° C., stirred for 15 min, and then 3 g of sodium dodecylbenzene sulfonate, 3 g of octylphenol polyoxyethylene ether OP-10 (Wuhan Glory Materials Co., Ltd.) and 36 g of water were added, and stirring was continued for 15 min.

[0062] After shearing with a shearing machine at a speed of 4000r / min for 10 minutes, it was placed in an oven at 65℃ for 30 minutes, sheared for another 10 minutes, and then placed in an oven at 65℃ for another 30 minutes.

[0063] Add 1g of sodium benzoate and 0.5g of essence, shear for 10 minutes, and let stand to room temperature to obtain a high-viscosity and high-elasticity modified asphalt bonding blocker 1, which is a milky white liquid.

[0064] Using the same method, the compound AdBlock-01 was replaced with rapeseed oil of equal mass to prepare a highly viscous and highly elastic modified asphalt bonding blocker 2, which was a milky white liquid;

[0065] Using the same method, the compound AdBlock-01 was replaced with an equal mass of cis-3-hexenyl hexanoate to prepare a highly viscous and highly elastic modified asphalt bonding blocker 3, which was a milky white liquid.

[0066] Using the same method, the compound AdBlock-01 was replaced with an equal mass of trans-2-hexenyl hexanoate to prepare a highly viscous and highly elastic modified asphalt bonding blocker 4, which was a milky white liquid.

[0067] Using the same method, an equal mass of cis-3-hexenoic acid cis-3-hexenyl ester was used to replace the compound AdBlock-01 to prepare a high-viscosity and high-elasticity modified asphalt bonding blocker 5, which was a milky white liquid.

[0068] Example 3: Evaluation of the effect of adhesion blockers on metal surface adhesion

[0069] Prepare the metal sample to be tested (20cm×20cm): Creusabro 4800 wear-resistant steel plate (Juxun special alloy). Clean the surface of the sample with water, keep the surface flat, and dry it.

[0070] Take high-viscosity and high-elastic modified asphalt (Type IB, Walter Road Materials) and heat it to melt. Place the metal sample on a horizontal table, and take 10g of the high-viscosity and high-elastic modified asphalt bonding blocker prepared as described in Example 2 and evenly apply it to the surface of the steel plate. Use a mold to shape the prepared asphalt melt, carefully pour it on the test area (8cm×8cm) of the metal sample and spread it all over. Let it stand at room temperature to allow the asphalt to solidify. Use a tensile tester (zwickiLine) to test the adhesion between the asphalt and the sample surface. The adhesion force is divided by the adhesion area to calculate the adhesion strength. Repeat the test 5 times and take the average result. As shown in Table 1.

[0071] Each bonding blocker has the effect of reducing the bonding between asphalt and metal. Among them, the adhesion strength of the bonding blocker group 1 with the compound AdBlock-01 added was much lower than that of the other groups, with a statistically significant difference (P<0.01). The bonding blocker group 5 was also significantly better than the bonding blocker group 2.

[0072] Table 1. Adhesion strength test on metal surfaces using bond blocking agents

[0073] Grouping Element Adhesion strength (MPa) No adhesive blocker none 0.495 Adhesion Blocker 1 Compound AdBlock-01 0.091 Adhesion Blocker 2 Rapeseed Oil 0.438 Adhesion Blocker 3 Cis-3-Hexenyl Hexanoate 0.424 Adhesion Blocker 4 Trans-2-Hexenyl Hexanoate 0.369 Adhesion Blocker 5 cis-3-Hexenoic acid cis-3-hexenyl ester 0.280

[0074] Example 4: Testing the effect of adhesion blocking agent on interlayer performance

[0075] According to the same method as the literature (Han Xiaozhou. Research on the development and application technology of new environmentally friendly asphalt isolation agent [D]. Chang'an University, 2016.), the interlayer bonding performance test was carried out to determine whether the bonding blocker has an effect on the interlayer performance.

[0076] First, AC-20 rutting plates (300*300*50mm) were formed. During the forming process, each group was evenly brushed with 30g of any bonding blocker prepared by the method described in Example 2, and then rolled and formed. After two days, 300g of the same hot asphalt adhesive layer was evenly brushed on it, and then AC-16 mid-surface layer was formed on it. After static pressure forming, core samples were drilled and the specimens were tested for tensile strength using a Proceq puller. The test was repeated 5 times and the results were averaged. The test results are shown in Table 2.

[0077] Table 2. Test results of the effect of adhesion blockers on interlayer performance

[0078]

[0079] When using bonding blocker 1 or bonding blocker 5, there was no significant difference in interlayer pull-out strength compared with the negative control group, indicating that it had no effect on the interlayer bonding function during pavement construction.

[0080] Although the embodiments of the present disclosure have been described above, it is understood that the above embodiments are exemplary and do not constitute limitations to the present invention. Those skilled in the art may change, modify and vary the above embodiments within the scope of the present invention.

Claims

1. A high-viscosity and high-elasticity modified asphalt adhesion blocking agent, characterized in that: The adhesion blocking agent comprises compound AdBlock-01 or cis-3-hexenoic acid cis-3-hexenyl ester, and the structure of the compound AdBlock-01 is:

2. The adhesion blocking agent according to claim 1, characterized in that The bonding blocker comprises the following ingredients by weight: 1% to 12% of dimethyl silicone oil, 1% to 14% of glycerol, 30% to 60% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% of sodium dodecylbenzene sulfonate, 1% to 5% of alkylphenol polyoxyethylene ether, a preservative, and the balance is water.

3. The adhesion blocking agent according to claim 1, characterized in that The preparation method of the bonding blocker is as follows: the main components are mixed, sheared at a speed of 4000r / min for 10 minutes using a shearing instrument, and then placed in an oven at 65°C for 30 minutes, sheared for another 10 minutes, and then placed in an oven at 65°C for another 30 minutes; preservatives and flavors are added, and then sheared for another 10 minutes, and then placed in an oven at 65°C for another 30 minutes; a high-viscosity and high-elasticity modified asphalt bonding blocker is obtained; The main components include the following components by weight: 1% to 12% of dimethyl silicone oil, 1% to 14% of glycerol, 30% to 60% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% of sodium dodecylbenzene sulfonate, 1% to 5% of alkylphenol polyoxyethylene ether OP-10, and an appropriate amount of water.

4. The adhesion blocking agent according to claim 1, characterized in that The preparation method of the adhesion blocking agent is as follows: 6g of dimethyl silicone oil, 12g of glycerol, and 40g of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate are mixed, heated to 65°C, stirred for 15min, and then 3g of sodium dodecylbenzene sulfonate, 3g of octylphenol polyoxyethylene ether OP-10 and 36g of water are added, and stirring is continued for 15min; after shearing with a shearing instrument at a speed of 4000r / min for 10min, the mixture is allowed to stand in an oven at 65°C for 30min, sheared for another 10min, and continued to stand in an oven at 65°C for 30min; 1g of sodium benzoate and 0.5g of essence are added, and the mixture is sheared for another 10min, and allowed to stand to room temperature to obtain the adhesion blocking agent.

5. The adhesion blocking agent according to claim 1, characterized in that The adhesion blocking agent blocks the adhesion between the high-viscosity and high-elasticity modified asphalt and the carriage of the transport vehicle, blocks the adhesion between the high-viscosity and high-elasticity modified asphalt and the receiving hopper of the paver, or blocks the adhesion between the high-viscosity and high-elasticity modified asphalt and the steel wheel of the roller.

6. A method for preparing a high-viscosity and high-elasticity modified asphalt adhesion blocking agent, characterized in that: The preparation method comprises the following steps: mixing the main components, shearing them with a shearing machine at a speed of 4000 r / min for 10 minutes, placing them in an oven at 65° C. for 30 minutes, shearing them for another 10 minutes, and placing them in an oven at 65° C. for another 30 minutes; adding preservatives and flavors, shearing them for another 10 minutes, and placing them in an oven at 65° C. for another 30 minutes; and obtaining a high-viscosity and high-elasticity modified asphalt bonding blocker. The main components include the following components by weight: 1% to 12% of dimethyl silicone oil, 1% to 14% of glycerol, 30% to 60% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% of sodium dodecylbenzene sulfonate, 1% to 5% of alkylphenol polyoxyethylene ether, and an appropriate amount of water; The structure of the compound AdBlock-01 is:

7. The preparation method according to claim 6, characterized in that: The main components include the following components by weight: 5% to 7% dimethicone, 10% to 14% glycerol, 30% to 50% of compound AdBlock-01 or cis-3-hexenyl hexanoate or trans-2-hexenyl hexanoate or cis-3-hexenyl cis-3-hexenoate, 1% to 5% sodium dodecylbenzene sulfonate, 1% to 5% octylphenol polyoxyethylene ether OP-10, and an appropriate amount of water.

8. Use of the adhesion blocking agent as described in any one of claims 1 to 5 in the transportation, paving and / or rolling of high-viscosity and high-elasticity modified asphalt mixture.

9. The use as claimed in claim 8, wherein the high-viscosity and high-elasticity modified asphalt mixture comprises high-viscosity and high-elasticity modified asphalt, coarse aggregate, fine aggregate, and mineral powder.

10. A compound having the structure:

Citation Information

Patent Citations

  • Asphalt separant and preparation method thereof

    CN105111936A

  • Anti-sticking separant for asphalt pavement roller and preparation method of the separant

    CN110128940A