Organic silicon packaging adhesive film with high light transmittance and preparation method thereof

By using silicone encapsulated films with high light transmittance in photovoltaic modules, the problems of low light transmittance and PID phenomena of photovoltaic modules are solved, and higher photoelectric conversion and lower power attenuation are achieved, which extends the The service life of the component.

CN118931413APending Publication Date: 2024-11-12ZHEJIANG DIMAI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411218082.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The light transmittance of existing photovoltaic module packaging films is low, resulting in low photoelectric conversion efficiency, and potential potential potential induced attenuation (PID) is prone to high temperature and high humidity environments, affecting power generation efficiency and investment recovery costs.

Method used

Using high-gloss transmittance silicone encapsulated film, including silicone film layer and primer, is prepared through specific formulas and processes to ensure that the light transmittance of the film is as high as 99%, and is in double 85, reverse 1000V, Maintain low power attenuation rate under 96h conditions.

Benefits of technology

It improves the photoelectric conversion rate by 1.5-3%, while effectively preventing PID phenomenon, maintains the aging resistance, temperature resistance and bonding properties of the silicone film, and extends the service life of photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005022139910000021
    Figure BDA0005022139910000021
  • Figure BDA0005022139910000022
    Figure BDA0005022139910000022
  • Figure BDA0005022139910000023
    Figure BDA0005022139910000023
Patent Text Reader

Abstract

The invention relates to an organic silicon packaging adhesive film with high light transmittance and a preparation method and application thereof, the packaging adhesive film comprises an organic silicon adhesive film layer and a priming coat, and the organic silicon adhesive film is an addition type organic silicon adhesive film. According to the packaging adhesive film, the excellent light transmittance, aging resistance, temperature resistance, yellowing resistance and weather resistance of organic silicon are reserved, the light transmittance reaches up to 99%, and the photoelectric conversion rate is increased by 1.5-3%; and meanwhile, a good anti-PID effect is achieved, and the power attenuation rate is smaller than or equal to 1.5% when a test is carried out under the conditions of double-85, reverse 1000V and 96h.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photovoltaic module packaging, and in particular to an organic silicon packaging film with high light transmittance and a preparation method thereof. Background Art

[0002] As a renewable green energy, solar energy has been developing rapidly around the world. Solar photovoltaic power generation is a technology that uses the photovoltaic effect of semiconductor interfaces to directly convert light energy into electrical energy. After the solar cells are connected in series, they are protected by glass, packaging materials and back panels, and finally frame sealants are injected and encapsulated with aluminum frames to form large-area photovoltaic modules.

[0003] Solar panels will produce PID (potential induced degradation) under high temperature and high humidity conditions. In a high temperature and high humidity environment, high voltage flowing through the solar cell unit will cause the output to drop. PID will reduce power generation efficiency and extend the time to pay back the investment cost. As one of the important factors affecting the power generation efficiency of photovoltaic panels, it is generally believed that the main external factors affecting the PID attenuation of the components are ambient temperature, ambient humidity, and the voltage transformer electric field between the alloy frame, glass and internal circuit of the system voltage.

[0004] At present, the most commonly used packaging films on the market are POE and EVA, which have low light transmittance, low photoelectric conversion efficiency, and low energy utilization. The light transmittance of traditional packaging materials after bonding is only about 90%, and nearly 10% of the light is not utilized, resulting in serious waste of resources. Studies have shown that an increase in light transmittance of 9% can increase the photoelectric conversion efficiency by 1.5-3%.

[0005] Organic silicon has excellent aging resistance, temperature resistance, electrical insulation and other properties. It also has a strong bonding effect on inorganic glass and organic backplanes, and the production process is simple. It is the best choice for encapsulation film. However, the film prepared by ordinary organic silicon addition reaction must use platinum, and the metal ions of platinum will cause serious PID phenomenon. How to solve the PID phenomenon and how to improve light transmittance are urgent problems to be solved in this field. Summary of the invention

[0006] Problem that the invention aims to solve

[0007] In view of the above problems existing in the prior art, an object of the present invention is to provide an organic silicon encapsulation film with high light transmittance.

[0008] Solutions for solving problems

[0009] The invention provides an organic silicone encapsulation film with high light transmittance. The encapsulation film comprises an organic silicone film layer and a primer layer. The organic silicone film is an addition-type organic silicone film.

[0010] Preferably, in parts by weight, the primer comprises:

[0011]

[0012] More preferably, in parts by weight, the primer comprises:

[0013]

[0014] Further preferably, in parts by weight, the primer comprises:

[0015]

[0016] Preferably, the thickness of the primer layer is 1-50 μm, preferably 45 μm.

[0017] Preferably, the acrylic monomer is selected from one or more of methyl methacrylate, hydroxyethyl methacrylate, 2-hydroxyethyl methacrylate, and propyl methacrylate. Preferably, the acrylic monomer is methyl methacrylate;

[0018] Preferably, the multifunctional polyurethane acrylate is an aliphatic polyurethane acrylate;

[0019] Preferably, the photoinitiator is selected from one or more of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO), and methyl benzoylformate. More preferably, the photoinitiator is 1-hydroxy-cyclohexyl phenyl ketone;

[0020] Preferably, the adhesion promoter is selected from one or more of 3-aminopropyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane. More preferably, the adhesion promoter is 3-glycidyloxypropyltrimethoxysilane.

[0021] Preferably, the organic silicone film is a two-component heat-curing adhesive;

[0022] Preferably, in parts by weight, the raw materials for preparing the organic silica gel film include:

[0023] Component A: 20-90 parts of vinyl silicone oil, 20-60 parts of vinyl silicone resin, 0.01-5 parts of platinum catalyst, and

[0024] Component B: 20-90 parts of vinyl silicone oil, 20-60 parts of vinyl silicone resin, 5-20 parts of crosslinking agent, and 0-2 parts of inhibitor.

[0025] Preferably, the vinyl silicone oil is a vinyl silicone oil with a viscosity of 10000 cst to 100000 cst. Preferably, the vinyl silicone oil is selected from one or more of RH-Vi301, RH-Vi302, and RH-Vi303.

[0026] Preferably, the vinyl silicone resin is a silicone resin having a vinyl content of 0.1-2 wt %, and more preferably, the vinyl silicone resin is selected from RH-S0836 and / or RH-S11H;

[0027] Preferably, the platinum catalyst is selected from one or more of divinyltetramethyldisiloxane platinum complex, divinyloctamethyltetrasiloxane platinum complex, and chloroplatinic acid-vinyl silicone oil solution. More preferably, the platinum catalyst is PT1003;

[0028] Preferably, the crosslinking agent is selected from one or more of terminal hydrogen silicone oil, side hydrogen silicone oil, and terminal side hydrogen-containing silicone oil. More preferably, the crosslinking agent is terminal side hydrogen-containing silicone oil. Further preferably, the crosslinking agent is RH-H86 and / or RH-H536.

[0029] Preferably, the inhibitor is selected from one or more of tetravinyltetramethylcyclotetrasiloxane, ethynylcyclohexanol, methylbutynol, and maleate. More preferably, the inhibitor is tetravinyltetramethylcyclotetrasiloxane.

[0030] The present invention also provides a method for preparing the encapsulating adhesive film, which comprises spraying the primer on a base film and coating the organic silicone film after curing.

[0031] Preferably, the method comprises:

[0032] (1) preparing the primer;

[0033] Preferably, the step (1) comprises:

[0034] (1a) mixing the acrylic monomer and multifunctional polyurethane acrylate;

[0035] (1b) After stirring evenly, adding a thickener;

[0036] (1c) After stirring evenly, add a photoinitiator;

[0037] (1d) After stirring evenly, vacuum degassing is performed to obtain the primer.

[0038] Preferably, the method further comprises:

[0039] (2) preparing the organic silica gel film;

[0040] Preferably, the step (2) comprises:

[0041] (2a) mixing the A components and stirring them evenly to obtain glue A;

[0042] (2b) mixing the B components and stirring them evenly to obtain B glue;

[0043] (2c) mixing glue A and glue B and curing them to obtain the organic silica gel film;

[0044] Preferably, the mass ratio of glue A to glue B is 1:1.

[0045] Preferably, the method further comprises:

[0046] (3) preparing the encapsulation film;

[0047] Preferably, the step (3) comprises:

[0048] (3a) spraying the primer prepared in step (1) onto the base film and performing a first curing;

[0049] (3b) coating the organic silicone film obtained in step (2), and curing it again to obtain the encapsulating film;

[0050] Preferably, the thickness of the primer is 1-50 μm, preferably 45 μm;

[0051] Preferably, the first curing is UV irradiation curing;

[0052] Preferably, the re-curing is a lamination curing.

[0053] The present invention also provides an application of the encapsulation adhesive film or the encapsulation adhesive film prepared according to the method in a solar module.

[0054] Effects of the Invention

[0055] The encapsulation film of the present invention retains the excellent light transmittance, aging resistance, temperature resistance, yellowing resistance and weather resistance of organic silicon, with a light transmittance of up to 99% and a photoelectric conversion rate increased by 1.5-3%. It also has a good anti-PID effect, and the power attenuation rate is ≤1.5% when tested under the conditions of double 85, reverse 1000V and 96h. DETAILED DESCRIPTION

[0056] In order to make the technical solutions and beneficial effects of the present invention more clearly understood, the following is a detailed description by listing specific embodiments. Unless otherwise defined, the technical and scientific terms used herein have the same meanings as those in the technical field to which this application belongs.

[0057] The invention provides an organic silicone encapsulation film with high light transmittance. The encapsulation film comprises an organic silicone film layer and a primer layer. The organic silicone film is an addition-type organic silicone film.

[0058] In certain embodiments, the primer comprises, by weight:

[0059]

[0060] In certain embodiments, the primer includes 10 parts, or 11 parts, or 12 parts, or 13 parts, or 14 parts, or 15 parts, or 16 parts, or 17 parts, or 18 parts, or 19 parts, or 20 parts, or 21 parts, or 22 parts, or 23 parts, or 24 parts, or 25 parts, or 26 parts, or 27 parts, or 28 parts, or 29 parts, or 30 parts, or 31 parts, or 32 parts, or 33 parts, or 34 parts, or 35 parts, or 36 parts, or 37 parts, or 38 parts, or 39 parts, or 40 parts of acrylic monomers, based on weight parts.

[0061] In certain embodiments, the primer includes 20 parts, or 21 parts, or 22 parts, or 23 parts, or 24 parts, or 25 parts, or 26 parts, or 27 parts, or 28 parts, or 29 parts, or 30 parts, or 31 parts, or 32 parts, or 33 parts, or 34 parts, or 35 parts, or 36 parts, or 37 parts, or 38 parts, or 39 parts, or 40 parts, or 41 parts, or 42 parts, based on weight parts. , or 43, or 44, or 45, or 46, or 47, or 48, or 49, or 50, or 51, or 52, or 53, or 54, or 55, or 56, or 57, or 58, or 59, or 60, or 61, or 62, or 63, or 64, or 65, or 66, or 67, or 68, or 69, or 70.

[0062] In certain embodiments, the primer includes 1 part, or 2 parts, or 3 parts, or 4 parts, or 5 parts, or 6 parts, or 7 parts, or 8 parts, or 9 parts, or 10 parts of the photoinitiator by weight.

[0063] In certain embodiments, the primer includes 1 part, or 2 parts, or 3 parts, or 4 parts, or 5 parts, or 6 parts, or 7 parts, or 8 parts, or 9 parts, or 10 parts of the adhesion promoter in parts by weight.

[0064] In certain embodiments, the primer comprises, by weight:

[0065]

[0066] In certain embodiments, the primer comprises, by weight:

[0067]

[0068] In certain embodiments, the primer layer has a thickness of 1-50 μm.

[0069] In certain embodiments, the thickness of the primer layer is 1 μm, or 2 μm, or 3 μm, or 4 μm, or 5 μm, or 6 μm, or 7 μm, or 8 μm, or 9 μm, or 10 μm, or 11 μm, or 12 μm, or 13 μm, or 14 μm, or 15 μm, or 16 μm, or 17 μm, or 18 μm, or 19 μm, or 20 μm, or 21 μm, or 22 μm, or 23 μm, or 24 μm, or 25 μm. 5μm, or 26μm, or 27μm, or 28μm, or 29μm, or 30μm, or 31μm, or 32μm, or 33μm, or 34μm, or 35μm, or 36μm, or 37μm, or 38μm, or 39μm, or 40μm, or 41μm, or 42μm, or 43μm, or 44μm, or 45μm, or 46μm, or 47μm, or 48μm, or 49μm, or 50μm.

[0070] In certain embodiments, the primer layer has a thickness of 30-50 μm.

[0071] In certain embodiments, the primer layer has a thickness of 45 μm.

[0072] In certain embodiments, the acrylic monomer is selected from one or more of methyl methacrylate, hydroxyethyl methacrylate, 2-hydroxyethyl methacrylate, and propyl methacrylate.

[0073] In certain embodiments, the acrylic monomer is methyl methacrylate, hydroxyethyl methacrylate, 2-hydroxyethyl methacrylate, and propyl methacrylate.

[0074] In certain embodiments, the acrylic monomer is methyl methacrylate, hydroxyethyl methacrylate, and 2-hydroxyethyl methacrylate.

[0075] In certain embodiments, the acrylic monomers are methyl methacrylate, hydroxyethyl methacrylate, and propyl methacrylate.

[0076] In certain embodiments, the acrylic monomer is hydroxyethyl methacrylate, 2-hydroxyethyl methacrylate, and propyl methacrylate.

[0077] In certain embodiments, the acrylic monomers are methyl methacrylate and hydroxyethyl methacrylate.

[0078] In certain embodiments, the acrylic monomers are methyl methacrylate and 2-hydroxyethyl methacrylate.

[0079] In certain embodiments, the acrylic monomers are methyl methacrylate and propyl methacrylate.

[0080] In certain embodiments, the acrylic monomers are hydroxyethyl methacrylate and 2-hydroxyethyl methacrylate.

[0081] In certain embodiments, the acrylic monomers are hydroxyethyl methacrylate and propyl methacrylate.

[0082] In certain embodiments, the acrylic monomers are 2-hydroxyethyl methacrylate and propyl methacrylate.

[0083] In certain embodiments, the acrylic monomer is methyl methacrylate.

[0084] In certain embodiments, the acrylic monomer is hydroxyethyl methacrylate.

[0085] In certain embodiments, the acrylic acid monomer is 2-hydroxyethyl methacrylate.

[0086] In certain embodiments, the acrylic monomer is propyl methacrylate.

[0087] In certain embodiments, the multifunctional urethane acrylate is an aliphatic urethane acrylate.

[0088] In certain embodiments, the photoinitiator is selected from one or more of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO), and methyl benzoylformate.

[0089] In certain embodiments, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, TPO and methyl benzoylformate.

[0090] In certain embodiments, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone and TPO.

[0091] In certain embodiments, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone and methyl benzoylformate.

[0092] In certain embodiments, the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone, TPO, and methyl benzoylformate.

[0093] In certain embodiments, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone and 2-hydroxy-2-methyl-1-phenyl-1-propanone.

[0094] In certain embodiments, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone and TPO.

[0095] In certain embodiments, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone and methyl benzoylformate.

[0096] In certain embodiments, the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone and TPO.

[0097] In certain embodiments, the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone and methyl benzoylformate.

[0098] In certain embodiments, the photoinitiator is TPO and methyl benzoylformate.

[0099] In certain embodiments, the photoinitiator is 1-hydroxy-cyclohexyl phenyl ketone.

[0100] In certain embodiments, the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.

[0101] In certain embodiments, the photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO).

[0102] In certain embodiments, the photoinitiator is methyl benzoylformate.

[0103] In certain embodiments, the adhesion promoter is selected from one or more of 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0104] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0105] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

[0106] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0107] In certain embodiments, the adhesion promoter is 3-glycidoxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0108] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0109] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0110] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-(methacryloyloxy)propyltrimethoxysilane.

[0111] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

[0112] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0113] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

[0114] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0115] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0116] In certain embodiments, the adhesion promoter is 3-glycidoxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

[0117] In certain embodiments, the adhesion promoter is 3-glycidoxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0118] In certain embodiments, the adhesion promoter is 3-glycidoxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0119] In certain embodiments, the adhesion promoter is 3-(methacryloyloxy)propyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane.

[0120] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane and 3-glycidoxypropyltrimethoxysilane.

[0121] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane and 3-(methacryloyloxy)propyltrimethoxysilane.

[0122] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0123] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane and 3-mercaptopropyltriethoxysilane.

[0124] In certain embodiments, the adhesion promoter is 3-glycidoxypropyltrimethoxysilane and 3-(methacryloyloxy)propyltrimethoxysilane.

[0125] In certain embodiments, the adhesion promoter is 3-glycidoxypropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0126] In certain embodiments, the adhesion promoter is 3-glycidoxypropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.

[0127] In certain embodiments, the adhesion promoter is 3-(methacryloyloxy)propyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0128] In certain embodiments, the adhesion promoter is 3-(methacryloyloxy)propyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.

[0129] In certain embodiments, the adhesion promoter is 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.

[0130] In certain embodiments, the adhesion promoter is 3-aminopropyltriethoxysilane.

[0131] In certain embodiments, the adhesion promoter is 3-glycidoxypropyltrimethoxysilane.

[0132] In certain embodiments, the adhesion promoter is 3-(methacryloyloxy)propyltrimethoxysilane

[0133] In certain embodiments, the adhesion promoter is 3-mercaptopropyltrimethoxysilane.

[0134] In certain embodiments, the adhesion promoter is 3-mercaptopropyltriethoxysilane.

[0135] In certain embodiments, the organic silicone film is a two-component thermal curing adhesive.

[0136] In certain embodiments, the raw materials for preparing the organic silica gel film include, by weight:

[0137] Component A: 20-90 parts of vinyl silicone oil, 20-60 parts of vinyl silicone resin, 0.01-5 parts of platinum catalyst, and

[0138] Component B: 20-90 parts of vinyl silicone oil, 20-60 parts of vinyl silicone resin, 5-20 parts of crosslinking agent, and 0-2 parts of inhibitor.

[0139] In certain embodiments, the A component includes 20 parts, or 21 parts, or 22 parts, or 23 parts, or 24 parts, or 25 parts, or 26 parts, or 27 parts, or 28 parts, or 29 parts, or 30 parts, or 31 parts, or 32 parts, or 33 parts, or 34 parts, or 35 parts, or 36 parts, or 37 parts, or 38 parts, or 39 parts, or 40 parts, or 41 parts, or 42 parts, or 43 parts, or 44 parts, or 45 parts, or 46 parts, or 47 parts, or 48 parts, or 49 parts, or 50 parts, or 51 parts, or 52 parts of vinyl silicone oil. , or 53, or 54, or 55, or 56, or 57, or 58, or 59, or 60, or 61, or 62, or 63, or 64, or 65, or 66, or 67, or 68, or 69, or 70, or 71, or 72, or 73, or 74, or 75, or 76, or 77, or 78, or 79, or 80, or 81, or 82, or 83, or 84, or 85, or 86, or 87, or 88, or 89, or 90.

[0140] In certain embodiments, the A component includes 20 parts, or 21 parts, or 22 parts, or 23 parts, or 24 parts, or 25 parts, or 26 parts, or 27 parts, or 28 parts, or 29 parts, or 30 parts, or 31 parts, or 32 parts, or 33 parts, or 34 parts, or 35 parts, or 36 parts, or 37 parts, or 38 parts, or 39 parts, or 40 parts, or 41 parts, or 42 parts, or 43 parts, or 44 parts, or 45 parts, or 46 parts, or 47 parts, or 48 parts, or 49 parts, or 50 parts, or 51 parts, or 52 parts, or 53 parts, or 54 parts, or 55 parts, or 56 parts, or 57 parts, or 58 parts, or 59 parts, or 60 parts of vinyl silicone resin.

[0141] In certain embodiments, the A component includes 0.01 parts, or 0.02 parts, or 0.03 parts, or 0.04 parts, or 0.05 parts, or 0.06 parts, or 0.07 parts, or 0.08 parts, or 0.09 parts, or 0.1 parts, or 0.2 parts, or 0.3 parts, or 0.4 parts, or 0.5 parts, or 0.6 parts, or 0.7 parts, or 0.8 parts, or 0.9 parts, or 1 part, or 2 parts, or 3 parts, or 4 parts, or 5 parts of platinum catalyst, by weight.

[0142] In certain embodiments, the component A includes, by weight, 78 parts of vinyl silicone oil, 21.5 parts of vinyl silicone resin, and 0.5 parts of platinum catalyst.

[0143] In certain embodiments, the component A includes, by weight, 44 parts of vinyl silicone oil, 49.5 parts of vinyl silicone resin, and 0.5 parts of platinum catalyst.

[0144] In certain embodiments, the B component includes 20 parts, or 21 parts, or 22 parts, or 23 parts, or 24 parts, or 25 parts, or 26 parts, or 27 parts, or 28 parts, or 29 parts, or 30 parts, or 31 parts, or 32 parts, or 33 parts, or 34 parts, or 35 parts, or 36 parts, or 37 parts, or 38 parts, or 39 parts, or 40 parts, or 41 parts, or 42 parts, or 43 parts, or 44 parts, or 45 parts, or 46 parts, or 47 parts, or 48 parts, or 49 parts, or 50 parts, or 51 parts, or 52 parts of vinyl silicone oil. , or 53, or 54, or 55, or 56, or 57, or 58, or 59, or 60, or 61, or 62, or 63, or 64, or 65, or 66, or 67, or 68, or 69, or 70, or 71, or 72, or 73, or 74, or 75, or 76, or 77, or 78, or 79, or 80, or 81, or 82, or 83, or 84, or 85, or 86, or 87, or 88, or 89, or 90.

[0145] In certain embodiments, the B component includes 20 parts, or 21 parts, or 22 parts, or 23 parts, or 24 parts, or 25 parts, or 26 parts, or 27 parts, or 28 parts, or 29 parts, or 30 parts, or 31 parts, or 32 parts, or 33 parts, or 34 parts, or 35 parts, or 36 parts, or 37 parts, or 38 parts, or 39 parts, or 40 parts, or 41 parts, or 42 parts, or 43 parts, or 44 parts, or 45 parts, or 46 parts, or 47 parts, or 48 parts, or 49 parts, or 50 parts, or 51 parts, or 52 parts, or 53 parts, or 54 parts, or 55 parts, or 56 parts, or 57 parts, or 58 parts, or 59 parts, or 60 parts of vinyl silicone resin.

[0146] In certain embodiments, the B component includes 5 parts, or 6 parts, or 7 parts, or 8 parts, or 9 parts, or 10 parts, or 11 parts, or 12 parts, or 13 parts, or 14 parts, or 15 parts, or 16 parts, or 17 parts, or 18 parts, or 19 parts, or 20 parts of the crosslinking agent by weight.

[0147] In certain embodiments, the B component includes 0 parts, or 0.1 parts, or 0.2 parts, or 0.3 parts, or 0.4 parts, or 0.5 parts, or 0.6 parts, or 0.7 parts, or 0.8 parts, or 0.9 parts, or 1 parts, or 1.1 parts, or 1.2 parts, or 1.3 parts, or 1.4 parts, or 1.5 parts, or 1.6 parts, or 1.7 parts, or 1.8 parts, or 1.9 parts, or 2 parts of the inhibitor, by weight.

[0148] In certain embodiments, the B component includes, by weight, 57.4 parts of vinyl silicone oil, 21.5 parts of vinyl silicone resin, 10 parts of a crosslinking agent, and 0.1 parts of an inhibitor.

[0149] In certain embodiments, the B component includes, by weight, 54 parts of vinyl silicone oil, 49.9 parts of vinyl silicone resin, 16 parts of crosslinking agent, and 0.1 parts of inhibitor.

[0150] In certain embodiments, the vinyl silicone oil is a vinyl silicone oil having a viscosity of 10000 cst to 100000 cst.

[0151] In certain embodiments, the vinyl silicone oil is selected from one or more of RH-Vi301, RH-Vi302, and RH-Vi303.

[0152] In certain embodiments, the vinyl silicone oil is RH-Vi301, RH-Vi302, and RH-Vi303.

[0153] In certain embodiments, the vinyl silicone oil is RH-Vi301 and RH-Vi302.

[0154] In certain embodiments, the vinyl silicone oil is RH-Vi301 and RH-Vi303.

[0155] In certain embodiments, the vinyl silicone oil is RH-Vi302 and RH-Vi303.

[0156] In certain embodiments, the vinyl silicone oil is RH-Vi301.

[0157] In certain embodiments, the vinyl silicone oil is RH-Vi302.

[0158] In certain embodiments, the vinyl silicone oil is RH-Vi303.

[0159] In certain embodiments, the vinyl silicone resin is a silicone resin having a vinyl content of 0.1-2 wt %.

[0160] In certain embodiments, the vinyl silicone resin is selected from RH-S0836 and / or RH-S11H.

[0161] In certain embodiments, the vinyl silicone resin is RH-S0836 and RH-S11H.

[0162] In certain embodiments, the vinyl silicone resin is RH-S0836.

[0163] In certain embodiments, the vinyl silicone resin is RH-S11H.

[0164] In certain embodiments, the platinum catalyst is selected from one or more of divinyltetramethyldisiloxane platinum complex, divinyloctamethyltetrasiloxane platinum complex, and chloroplatinic acid-vinyl silicone oil solution.

[0165] In certain embodiments, the platinum catalyst is PT1003.

[0166] In certain embodiments, the crosslinking agent is selected from one or more of terminal hydrogen silicone oil, pendant hydrogen silicone oil, and terminal and side hydrogen-containing silicone oil.

[0167] In certain embodiments, the cross-linking agent is terminal hydrogen-containing silicone oil.

[0168] In certain embodiments, the cross-linking agent is RH-H86 and / or RH-H536.

[0169] In certain embodiments, the cross-linking agents are RH-H86 and RH-H536.

[0170] In certain embodiments, the cross-linking agent is RH-H86.

[0171] In certain embodiments, the cross-linking agent is RH-H536.

[0172] In certain embodiments, the inhibitor is selected from one or more of tetravinyltetramethylcyclotetrasiloxane, ethynylcyclohexanol, methylbutynol, and maleic acid esters.

[0173] In certain embodiments, the inhibitor is tetravinyltetramethylcyclotetrasiloxane.

[0174] The present invention also provides a method for preparing the encapsulating adhesive film, which comprises spraying the primer on a base film and coating the organic silicone film after curing.

[0175] In certain embodiments, the method comprises:

[0176] (1) Prepare the primer.

[0177] In certain embodiments, the step (1) comprises:

[0178] (1a) mixing the acrylic monomer and multifunctional polyurethane acrylate;

[0179] (1b) After stirring evenly, adding a thickener;

[0180] (1c) After stirring evenly, add a photoinitiator;

[0181] (1d) After stirring evenly, vacuum degassing is performed to obtain the primer.

[0182] In certain embodiments, the acrylic acid monomer in step (1a) is methyl methacrylate.

[0183] In certain embodiments, the multifunctional urethane acrylate in step (1a) is aliphatic urethane acrylate.

[0184] In certain embodiments, the adhesion promoter in step (1b) is 3-glycidyloxypropyltrimethoxysilane.

[0185] In certain embodiments, the photoinitiator in step (1c) is 1-hydroxy-cyclohexyl phenyl ketone.

[0186] In certain embodiments, the method further comprises:

[0187] (2) Preparing the organic silica gel film.

[0188] In certain embodiments, the step (2) comprises:

[0189] (2a) mixing the A components and stirring them evenly to obtain glue A;

[0190] (2b) mixing the B components and stirring them evenly to obtain B glue;

[0191] (2c) Glue A and glue B are mixed and cured to obtain the organic silicone film.

[0192] In certain embodiments, the mixing in step (2a) is performed in a vacuum kneader for half an hour.

[0193] In certain embodiments, the mixing in step (2b) is performed in a vacuum kneader for half an hour.

[0194] In certain embodiments, the mass ratio of glue A to glue B is 1:1.

[0195] In certain embodiments, the curing in step (2c) is performed at 120°C / 30 min or at room temperature for 24 h.

[0196] In certain embodiments, the curing in step (2c) is performed at 120° C. for 30 min.

[0197] In certain embodiments, the curing in step (2c) is performed at room temperature for 24 hours.

[0198] In certain embodiments, the method further comprises:

[0199] (3) Preparing the encapsulation film.

[0200] In certain embodiments, step (3) comprises:

[0201] (3a) spraying the primer prepared in step (1) onto the base film and performing a first curing;

[0202] (3b) coating the organic silicone film obtained in step (2), and curing it again to obtain the encapsulating adhesive film.

[0203] In certain embodiments, the primer has a thickness of 1-50 μm.

[0204] In certain embodiments, the thickness of the primer is 1 μm, or 2 μm, or 3 μm, or 4 μm, or 5 μm, or 6 μm, or 7 μm, or 8 μm, or 9 μm, or 10 μm, or 11 μm, or 12 μm, or 13 μm, or 14 μm, or 15 μm, or 16 μm, or 17 μm, or 18 μm, or 19 μm, or 20 μm, or 21 μm, or 22 μm, or 23 μm, or 24 μm, or 25 μm. 5μm, or 26μm, or 27μm, or 28μm, or 29μm, or 30μm, or 31μm, or 32μm, or 33μm, or 34μm, or 35μm, or 36μm, or 37μm, or 38μm, or 39μm, or 40μm, or 41μm, or 42μm, or 43μm, or 44μm, or 45μm, or 46μm, or 47μm, or 48μm, or 49μm, or 50μm.

[0205] In certain embodiments, the primer has a thickness of 30-50 μm.

[0206] In certain embodiments, the primer has a thickness of 45 μm.

[0207] In certain embodiments, the first curing is UV irradiation curing.

[0208] In certain embodiments, the first curing is performed by irradiating with a UV lamp for 30 seconds.

[0209] In certain embodiments, the re-curing is a lamination cure.

[0210] In certain embodiments, the re-curing is performed at 120-150° C. for 30 min.

[0211] In certain embodiments, the re-curing is curing at 120° C. for 30 min.

[0212] The present invention also provides an application of the encapsulation adhesive film or the encapsulation adhesive film prepared according to the method in a solar module.

[0213] In certain embodiments, the solar module comprises a solar cell.

[0214] Example 1: Preparation of organic silica gel film 1

[0215] Preparation of raw materials (by weight):

[0216] Component A:

[0217] Vinyl silicone oil (RH-Vi302): 78 parts

[0218] Vinyl silicone resin (RH-S0836): 21.5 parts

[0219] Platinum catalyst (PT1003): 0.5 parts

[0220] Component B:

[0221] Vinyl silicone oil (RH-Vi302): 57.4 parts

[0222] Vinyl silicone resin (RH-S0836): 21.5 parts

[0223] Hydrogenated silicone oil (RH-H86): 10 parts

[0224] Inhibitor (tetravinyltetramethylcyclotetrasiloxane, MVC): 0.1 parts

[0225] Preparation method:

[0226] 1. Add vinyl silicone oil, vinyl silicone resin and platinum catalyst into a vacuum kneader and blend for half an hour to obtain glue A.

[0227] 2. Add vinyl silicone oil, vinyl silicone resin, hydrogenated silicone oil and inhibitor into a vacuum kneader and blend for half an hour to obtain glue B.

[0228] 3. Mix glue A and glue B in a mass ratio of 1:1 and cure them at 120℃ / 30min or room temperature for 24h to obtain an organic silicone film.

[0229] Viscometer (DVPL) test: Use 14# rotor, 10rpm to test the viscosity. The results show that the viscosity of glue A is 15000mpa.s; the viscosity of glue B is 13000mpa.s.

[0230] Anton rheometer test: The organic silica gel film prepared in Example 1 was tested using a CP25 rotor, 120°C, a rotation speed of 1 rad / s, and a gel time of 12 min. The results showed that the storage modulus was 20452 Pa and the loss modulus was 864 Pa.

[0231] Optical transmittance: tested with optical transmittance meter YT1010 (Sanshi) according to GB / T2410 national standard, visible light 380nm-760nm, glue A / glue B mixed in a mass ratio of 1:1, use 18*18*2mm square mold to prepare the sample, put it in a 120℃ oven for curing, and test at room temperature and 50% humidity. The results show that the light transmittance is 99.2%.

[0232] Example 2: Preparation of organic silica gel film 2

[0233] Preparation of raw materials (by weight):

[0234] Component A:

[0235] Vinyl silicone oil 1 (RH-Vi301): 20 parts

[0236] Vinyl silicone oil 2 (RH-Vi303): 24 parts

[0237] Vinyl silicone resin (RH-S11H): 49.5 parts

[0238] Platinum catalyst (PT1003): 0.5 parts

[0239] Component B:

[0240] Vinyl silicone oil 1 (RH-Vi301): 30 parts

[0241] Vinyl silicone oil 2 (RH-Vi303): 24 parts

[0242] Vinyl silicone resin (RH-S11H): 49.9 parts

[0243] Hydrogenated silicone oil (RH-H536): 16 parts

[0244] Inhibitor (tetravinyltetramethylcyclotetrasiloxane, MVC): 0.1 parts

[0245] Preparation method:

[0246] 1. Add vinyl silicone oil 1, vinyl silicone oil 2, vinyl silicone resin and platinum catalyst into a vacuum kneader and blend for half an hour to obtain glue A.

[0247] 2. Add vinyl silicone oil 1, vinyl silicone oil 2, vinyl silicone resin, hydrogen-containing silicone oil and inhibitor into a vacuum kneader and blend for half an hour to obtain glue B.

[0248] 3. Mix glue A and glue B in a mass ratio of 1:1 and cure them at 120℃ / 30min or room temperature for 24h to obtain an organic silicone film.

[0249] Viscometer (DVPL) test: Use 14# rotor, 10rpm to test the viscosity. The results show that the viscosity of glue A is 17000mpa.s, and the viscosity of glue B is 15000mpa.s.

[0250] Anton Rheometer Test: The organic silica film prepared in step 3 was tested using a CP25 rotor, 120°C, a rotation speed of 1 rad / s, and a gel time of 7 minutes. The results showed that the storage modulus was 30278 Pa and the loss modulus was 795 Pa.

[0251] Optical transmittance: tested with optical transmittance meter YT1010 (Sanshi) according to GB / T2410 national standard, visible light 380nm-760nm, glue A / glue B mixed in a mass ratio of 1:1, use 18*18*2mm square mold to prepare the sample, put it in a 120℃ oven for curing, and test at room temperature and 50% humidity. The results show that the light transmittance is 99.1%.

[0252] Example 3: Preparation of packaging film

[0253] Primer preparation raw materials:

[0254] Methyl methacrylate: 20%

[0255] Aliphatic polyurethane acrylate: 66%

[0256] 1-Hydroxy-cyclohexylphenyl ketone: 8%

[0257] 3-Glycidyloxypropyltrimethoxysilane: 6%

[0258] Preparation method:

[0259] 1. Mix methyl methacrylate and aliphatic polyurethane acrylate and stir evenly;

[0260] 2. Add 3-glycidyloxypropyltrimethoxysilane as a tackifier and continue stirring;

[0261] 3. After stirring evenly, add the photoinitiator 1-hydroxy-cyclohexyl phenyl ketone and continue stirring;

[0262] 4. After stirring evenly, vacuum degassing is performed to obtain the primer.

[0263] The primer was sprayed on the base film with a thickness of 45 μm, and cured by UV lamp for 30 seconds, and then coated with organic silicone film 1, cured by laminator, and cured for 30 minutes at 120°C to obtain the encapsulation film. The encapsulation film was subjected to PID test, and the results showed that the PID value was 1.5% under the conditions of double 85, reverse 1000V, and 96h.

[0264] The primer was sprayed on the base film with a thickness of 45 μm, and cured by UV lamp for 30 seconds, and then coated with organic silicone film 2, and cured by laminator at 120°C for 30 minutes to obtain the encapsulation film. The encapsulation film was tested for PID, and the results showed that the PID value was 1.2% under the conditions of double 85, reverse 1000V, and 96h.

[0265] Comparative Example 1: Encapsulation film without primer

[0266] The organic silicone film 1 was coated on the base film and cured by a laminator at 120°C for 30 minutes. Then a PID test was performed. Under the conditions of double 85, reverse 1000V, and 96h, the results showed that the PID value was 24.5%.

[0267] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.

Claims

1. A high light transmittance silicone encapsulation film, It is characterized in that The encapsulation film comprises an organic silicone film layer and a primer layer, and the organic silicone film is an addition-type organic silicone film.

2. The encapsulation film according to claim 1, It is characterized in that In parts by weight, the primer comprises: Preferably, in parts by weight, the primer comprises: More preferably, in parts by weight, the primer comprises: Preferably, the thickness of the primer layer is 1-50 μm, preferably 45 μm.

3. The encapsulation film according to claim 2, It is characterized in that The acrylic acid monomer is selected from one or more of methyl methacrylate, hydroxyethyl methacrylate, 2-hydroxyethyl methacrylate, and propyl methacrylate. Preferably, the acrylic acid monomer is methyl methacrylate; Preferably, the multifunctional polyurethane acrylate is an aliphatic polyurethane acrylate; Preferably, the photoinitiator is selected from one or more of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO), and methyl benzoylformate. More preferably, the photoinitiator is 1-hydroxy-cyclohexyl phenyl ketone; Preferably, the adhesion promoter is selected from one or more of 3-aminopropyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyltriethoxysilane. More preferably, the adhesion promoter is 3-glycidyloxypropyltrimethoxysilane.

4. The encapsulation film according to claim 1, It is characterized in that The organic silicone film is a two-component heat-curing adhesive; Preferably, in parts by weight, the raw materials for preparing the organic silica gel film include: Component A: 20-90 parts of vinyl silicone oil, 20-60 parts of vinyl silicone resin, 0.01-5 parts of platinum catalyst, and Component B: 20-90 parts of vinyl silicone oil, 20-60 parts of vinyl silicone resin, 5-20 parts of crosslinking agent, and 0-2 parts of inhibitor.

5. The encapsulation film according to claim 4, It is characterized in that The vinyl silicone oil is a vinyl silicone oil with a viscosity of 10000 cst to 100000 cst. Preferably, the vinyl silicone oil is selected from one or more of RH-Vi301, RH-Vi302, and RH-Vi303; Preferably, the vinyl silicone resin is a silicone resin having a vinyl content of 0.1-2 wt %, and more preferably, the vinyl silicone resin is selected from RH-S0836 and / or RH-S11H; Preferably, the platinum catalyst is selected from one or more of divinyltetramethyldisiloxane platinum complex, divinyloctamethyltetrasiloxane platinum complex, and chloroplatinic acid-vinyl silicone oil solution. More preferably, the platinum catalyst is PT1003; Preferably, the crosslinking agent is selected from one or more of terminal hydrogen silicone oil, side hydrogen silicone oil, and terminal side hydrogen-containing silicone oil. More preferably, the crosslinking agent is terminal side hydrogen-containing silicone oil. Further preferably, the crosslinking agent is RH-H86 and / or RH-H536. Preferably, the inhibitor is selected from one or more of tetravinyltetramethylcyclotetrasiloxane, ethynylcyclohexanol, methylbutynol, and maleate. More preferably, the inhibitor is tetravinyltetramethylcyclotetrasiloxane.

6. A method for preparing a packaging film according to any one of claims 1 to 5, It is characterized in that The method comprises spraying the primer on a base film, and coating the organic silicone film after curing.

7. The method according to claim 6, It is characterized in that The method comprises: (1) preparing the primer; Preferably, the step (1) comprises: (1a) mixing the acrylic monomer and multifunctional polyurethane acrylate; (1b) After stirring evenly, adding a thickener; (1c) After stirring evenly, add a photoinitiator; (1d) After stirring evenly, vacuum degassing is performed to obtain the primer.

8. The method according to claim 7, It is characterized in that The method further comprises: (2) preparing the organic silica gel film; Preferably, the step (2) comprises: (2a) mixing the A components and stirring them evenly to obtain glue A; (2b) mixing the B components and stirring them evenly to obtain B glue; (2c) mixing glue A and glue B and curing them to obtain the organic silica gel film; Preferably, the mass ratio of glue A to glue B is 1:

1.

9. The method according to claim 8, It is characterized in that The method further comprises: (3) preparing the encapsulation film; Preferably, the step (3) comprises: (3a) spraying the primer prepared in step (1) onto the base film and performing a first curing; (3b) coating the organic silicone film obtained in step (2), and curing it again to obtain the encapsulating film; Preferably, the thickness of the primer is 1-50 μm, preferably 45 μm; Preferably, the first curing is UV irradiation curing; Preferably, the re-curing is a lamination curing.

10. Use of the encapsulation film according to any one of claims 1 to 5, or the encapsulation film prepared by the method according to any one of claims 5 to 9 in a solar module.