Lithium ion battery diaphragm coating binder, lithium-rich diaphragm, preparation method of lithium-rich diaphragm and battery
By adding a specific proportion of lithium sodium carboxymethylcellulose salt to the lithium-ion battery separator and using zirconium oxide, lanthanum, and copper catalysts to form a lithium-rich separator, the problem of lithium ion consumption during the first charging and discharging of lithium-ion batteries is solved. , improves the electrochemical performance and stability of the battery, reduces cost and deintercalation efficiency.
Patent Information
- Application Number
- CN202410977569.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
The solid electrolyte interface (SEI) film formed by lithium-ion batteries during the first charging and discharging process leads to lithium ion consumption, reducing the initial capacity and efficiency of the battery. The prior art is difficult to effectively solve and may affect other battery performance or increase the preparation cost.
By adding a specific proportion of lithium sodium carboxymethylcellulose salt to the lithium-ion battery separator coating adhesive, the ionic conductivity, permeability and bonding properties of the separator are optimized, using zirconia, lanthanum and copper as catalysts. Accurately control the ratio of lithium and sodium ions to form a lithium-rich separator to supplement the irreversible loss of lithium ions.
It improves the electrochemical performance, stability and safety of the battery, reduces the battery production cost, extends the cycle life, reduces the deintercalation efficiency of lithium ions, and improves the fast charging performance and performance stability of the battery.
Smart Images

Figure BDA0004955026250000071 
Figure BDA0004955026250000081 
Figure BDA0004955026250000082
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery separators, and in particular to a lithium-ion battery separator coated with a binder, a lithium-rich separator, a preparation method thereof, and a battery. Background Art
[0002] With the development of science and technology, batteries are being used more and more widely. Among them, lithium-ion batteries are widely used in various electronic devices, electric vehicles and other fields due to their high energy density, long cycle life and environmental protection. However, during the first charge and discharge process of lithium-ion batteries, a solid electrolyte interface (SEI) film will form on the negative electrode. This process will consume some lithium ions, thereby reducing the initial capacity and efficiency of the battery. Therefore, how to effectively solve this problem and improve battery performance is one of the important research directions in the current field of battery manufacturing technology.
[0003] In order to solve this problem, the existing technology mainly reduces the formation of SEI film and thus reduces the consumption of lithium ions by improving the formula of the electrolyte or adding some additives to the electrolyte. However, the method of improving the electrolyte may affect other properties of the battery, such as the stability of the electrolyte and the safety of the battery. There are also some technologies that improve the initial efficiency of the battery by changing the composition of the electrode material or optimizing the preparation process of the electrode. However, it will lead to the preparation cost of the battery, which is not conducive to large-scale production. The Japanese patent application number JP1996027910 discloses a method of preparing a lithium-ion battery by covering the surface of the negative electrode with a metal lithium sheet, then winding it into a battery, and then perfusing the electrolyte. Although this method can also play a role in replenishing lithium, the amount of lithium that the negative electrode can absorb is far less than the lithium provided by the metal lithium sheet, so it will cause uneven lithium insertion and deformation of the electrode sheet, and lithium precipitation is also prone to occur in subsequent cycles.
[0004] There are relatively few reports on lithium replenishment of diaphragms. The Chinese patent with publication number CN105932206A discloses a lithium replenishment composite diaphragm, which first coats a ceramic layer on the surface of a porous base membrane, and then introduces a lithium-containing layer. However, the surface of the metal lithium layer does not contain a protective layer, and the lithium layer will react when in contact with the environment, which may cause part of the active lithium to be deactivated and even cause safety risks. The Chinese patent with publication number CN113851786A provides a pre-lithiation composite diaphragm, which can effectively improve the first efficiency of lithium-ion batteries, thereby increasing the energy density of the battery, and the degree of pre-lithiation is controllable, but as a new technology, the long-term and reliability of the pre-lithiation composite diaphragm still need further verification. The Chinese patent with publication number CN117186616A discloses a diaphragm composition and an aerogel solid electrolyte diaphragm. Through lithium ion intercalation, disulfide metal compounds can not only serve as excellent ion conductors to increase the migration number of lithium ions and thus improve battery performance, but can also serve as lithium-rich materials to compensate for the loss of lithium ions and increase battery capacity. However, during long-term charge and discharge cycles, the stability of the disulfide metal compounds may be affected, which may lead to a decrease in the migration number of lithium ions and a decay of the battery capacity. In addition, the special preparation process and conditions will increase the difficulty and complexity of processing.
[0005] Therefore, a better technical solution is needed to solve the problem of reducing the battery capacity reduction caused by the irreversible capacity of the battery during the first charge and discharge process. Summary of the invention
[0006] In order to reduce the reduction in battery capacity caused by the irreversible capacity of the battery during the first charge and discharge process, the present invention provides a lithium-ion battery diaphragm coating binder, a lithium-rich diaphragm and a preparation method thereof and a battery. By adding a carboxymethyl cellulose salt with a specific lithium-sodium ratio as a lithium-rich binder into the coating diaphragm system, the irreversible loss of lithium ions caused by the first charge is supplemented to ensure the energy density of the battery.
[0007] In order to achieve the above object, the present invention provides a first aspect of a lithium ion battery separator coating binder, wherein the chemical formula of the lithium ion battery separator coating binder is [C6H7O2(OH)2OCH2COONa x Li 1-x ] n , where 0.75≤x≤0.80, and n is a natural number greater than 0.
[0008] A typical example is [C6H7O2(OH)2OCH2COONa 0.75 Li 0.25 ] n 、[C6H7O2(OH)2OCH2COONa 0.76 Li 0.24 ] n、[C6H7O2(OH)2OCH2COONa 0.77 Li 0.23 ] n 、[C6H7O2(OH)2OCH2COONa 0.78 Li 0.22 ] n 、[C6H7O2(OH)2OCH2COONa 0.79 Li 0.21 ] n 、[C6H7O2(OH)2OCH2COONa 0.80 Li 0.20 ] n wait.
[0009] By precisely controlling the ratio of lithium and sodium ions in the binder CMC, not only the ionic conductivity of the separator is improved, which helps maintain the ionic permeability of the separator and ensures that the ions in the electrolyte can be efficiently transmitted, but also the bonding performance of the separator is optimized, thereby improving the electrochemical performance of the battery. In addition, the specific ratio improves the rheological properties of the slurry, which helps reduce the risk of thermal runaway inside the battery. Specifically:
[0010] 1. Improve ion conductivity: The specific ratio has good electronic and ionic conductivity, which can promote the transfer of lithium ions and increase the migration rate of ions in the electrolyte, thereby enhancing the ionic conductivity of the separator.
[0011] Maintaining ion permeability (diaphragm permeability): A specific ratio can stabilize the interface structure inside the battery, prevent Li agglomeration, help maintain the stability of the internal structure of the battery, and provide a good channel for the migration of ions in the electrolyte. The membrane permeability can be expressed by the membrane permeability data.
[0012] The appropriate ratio of sodium ions to lithium ions (sodium: lithium = 75:25-80:20) can not only improve the ionic conductivity of the diaphragm, but also help maintain the ionic permeability of the diaphragm. When the sodium-to-lithium ratio is less than this ratio, the low sodium salt content has an adverse effect on the ionic permeability of the diaphragm, causing a significant increase in the permeability of the diaphragm; when the sodium-to-lithium ratio is greater than this ratio, the low lithium salt content leads to a small increase in ionic conductivity.
[0013] 2. Optimize bonding performance: Linear polymers with a specific structure and certain plasticity can stabilize the interface structure between the diaphragm and the electrode and prevent the collapse of the electrolyte structure on the interface.
[0014] The appropriate ratio of sodium ions to lithium ions (sodium: lithium = 75:25-80:20) can ensure excellent bonding performance. When the sodium-to-lithium ratio is less than this ratio and contains a lower concentration of sodium ions, the slurry viscosity will be reduced, affecting the bonding performance; when the sodium-to-lithium ratio is greater than this ratio and contains a higher concentration of sodium ions, the slurry viscosity will be increased, resulting in uneven thickness and surface density during coating, affecting the coating effect.
[0015] 3. Improve rheological properties: The addition of Li ions will interact with CMC molecules to form a network structure, which can increase the viscosity and stability of the slurry. At high shear rates, the viscosity of the slurry will decrease, which is beneficial to the coating process.
[0016] The appropriate ratio of sodium ions to lithium ions (sodium: lithium = 75:25-80:20) can effectively improve the rheological properties of the slurry. When the sodium-lithium ratio is less than this ratio, it affects [C6H7O2(OH)2OCH2COONa x Li 1-x ] n of water solubility and cannot be evenly distributed in water during the preparation process; when the sodium-to-lithium ratio is greater than this ratio and contains a higher concentration of sodium ions, the sodium ions will form an electric field double layer with the negative charges on the particle surface, reducing the absolute value of the particle surface charge, weakening the electrostatic repulsion on the particle surface, and increasing the attraction between particles, thereby increasing the slurry viscosity and reducing fluidity.
[0017] The second aspect of the present invention provides a method for preparing the above-mentioned lithium ion battery separator coating binder, comprising the following steps:
[0018] (1) Provide sodium carboxymethyl cellulose CMC-Na ([C6H7O2(OH)2OCH2COONa] n );
[0019] (2) CMC-Na and a lithium source are mixed according to a sodium to lithium molar ratio of 75:25-80:20 in each repeating unit, and a solvent is added to form a reaction mixture; a catalyst is then added to the reaction mixture, and the reaction is carried out under a constant temperature condition; after the reaction is completed, a precipitant is added, and the lithium ion battery separator coating binder [C6H7O2(OH)2OCH2COONa is obtained after filtering, washing, and drying. x Li 1-x ] n , wherein 0.75≤x≤0.80, n is a natural number greater than 0; wherein the catalyst is composed of zirconium oxide, lanthanum powder and copper powder, the molar ratio of zirconium oxide, lanthanum powder and copper powder is 50-70:10-20:20-30, and the total molar amount of lanthanum powder and copper powder is the same as the molar amount of lithium.
[0020] Step (1):
[0021] The purity of CMC-Na is ≥99.9%, and it can be purchased from the market or prepared by oneself.
[0022] In some embodiments, the preparation method of CMC-Na comprises the following steps:
[0023] a. Alkalization: the crushed refined cotton is put into a reactor filled with isopropanol-tert-butanol solvent, 30-55% sodium hydroxide aqueous solution is added with stirring, and alkalization is carried out at room temperature for 40-120 minutes; the mass ratio of isopropanol and tert-butanol in the isopropanol-tert-butanol solvent is 75:25;
[0024] b. Etherification: add 50-80% chloroacetic acid aqueous solution, react at 25-30 ° C for 30-40 minutes, heat to 55-60 ° C and react for 50-60 minutes, cool to room temperature; wherein the mass ratio of refined cotton: sodium hydroxide: chloroacetic acid is 20-30:30-40:30-40;
[0025] c. Purification: After neutralization with hydrochloric acid, filter, wash with ethanol 3-5 times, dry and crush to obtain CMC-Na.
[0026] Step (2):
[0027] In some embodiments, the lithium source is lithium hydroxide or lithium carbonate.
[0028] In some embodiments, the solvent is water, and the solid-liquid ratio is 100 g: 300-400 mL.
[0029] In some embodiments, the reaction temperature is 75-80° C., the reaction time is 6-7 hours, and the pH is 9-10.
[0030] The present invention selects specific catalysts, among which zirconium oxide, as a material with high thermal stability and chemical stability, is used as a catalyst carrier, and the lattice has different phase changes, which have a significant effect on the performance of the catalyst; the introduction of lanthanum can change the electronic structure and surface active sites of the catalyst, thereby improving the catalytic activity and selectivity; copper as a metal catalyst can further enhance the activity and selectivity of the catalyst.
[0031] Under the action of the above catalyst, the CMC-Na molecules interact with the active sites on the catalyst surface, causing the sodium ions in the CMC-Na molecules to be replaced or substituted by the lanthanum and copper ions in the catalyst according to a preset ratio. When lithium hydroxide is added, the lithium ions occupy the positions of copper and lanthanum, and copper and lanthanum form copper hydroxide and lanthanum hydroxide respectively under the action of the precipitant. Zirconium oxide in the catalyst can stabilize the catalyst structure and promote ion exchange. At the same time, the catalytic activity of lanthanum and copper helps to reduce the activation energy of the reaction, accelerate the ion exchange process, and make it react completely.
[0032] The copper ions and lanthanum ions are precipitated into solid particles by chemical reaction. Commonly used precipitants include sodium hydroxide, calcium hydroxide, etc., which can react with copper ions and lanthanum ions to form insoluble precipitates, such as copper hydroxide and lanthanum hydroxide. These precipitates can be separated from the solution by filtration or centrifugation.
[0033] The present invention provides a new preparation method capable of accurately regulating the lithium-sodium ratio, and the lithium-sodium ratio in the binder is accurately regulated by controlling the molar ratio of added CMC-Na to lithium hydroxide raw material.
[0034] The third aspect of the present invention provides a lithium-rich diaphragm, including a base film and a lithium-rich ceramic coating, the lithium-rich ceramic coating including ceramic powder, and the above-mentioned lithium-ion battery diaphragm coating binder or the lithium-ion battery diaphragm coating binder prepared by the above-mentioned preparation method.
[0035] The base film can be a polyethylene microporous film, a polypropylene microporous film, a polyethylene / polypropylene / polyethylene three-layer composite microporous film, a polyvinylidene fluoride microporous film, a polyimide microporous film, a non-woven fabric, etc., but is not limited thereto. There is no particular restriction on the thickness of the base film. Generally speaking, the thickness is less than 20 μm, for example, it can be 4-20 μm. There is no particular restriction on the pore size and porosity of the base film, as long as it is suitable for use as a separator for a lithium battery, for example, the porosity can be 40-55%. There is no particular restriction on the air permeability of the base film, as long as it is suitable for use as a separator for a lithium battery, for example, the air permeability can be 50-500s / 100cc.
[0036] The ceramic powder can be at least one selected from silicon dioxide (SiO2), aluminum oxide (Al2O3), magnesium oxide (MgO), zirconium oxide (ZrO2), titanium oxide (TiO2), calcium oxide (CaO), boehmite (ALOOH), aluminum nitride (AlN), boron nitride (BN), barium sulfate (BaSO4), calcium fluoride (CaF2), barium fluoride (BaF2), and barium titanate (BaTiO3).
[0037] A fourth aspect of the present invention provides a method for preparing the above-mentioned lithium-rich separator, comprising the following steps:
[0038] (1) dissolving the above-mentioned lithium ion battery separator coating binder in water to prepare a binder solution with a solid content of 3%-5%;
[0039] (2) 40 to 60 parts by weight of water, 0.3 to 0.5 parts by weight of a dispersant (such as a polycarboxylate), 30 to 40 parts by weight of a ceramic powder, 10 to 20 parts by weight of the binder solution, 5 to 10 parts by weight of a polyacrylate, and 0.005 to 0.01 parts by weight of a wetting agent (such as a polyether-modified polysiloxane) are mixed to prepare a slurry;
[0040] (3) The prepared slurry is coated on the base film and dried to obtain a lithium-rich separator.
[0041] A fifth aspect of the present invention provides a battery, comprising the lithium-rich diaphragm mentioned above or the lithium-rich diaphragm prepared by the above preparation method.
[0042] Beneficial effects:
[0043] (1) The present invention not only improves the ionic conductivity of the diaphragm and helps maintain the ionic permeability of the diaphragm by precisely controlling the ratio of lithium and sodium ions in the binder CMC, but also provides stronger bonding force, helps maintain the stability of the battery structure, and thus improves the electrochemical performance of the battery.
[0044] (2) By increasing the proportion of lithium ions in CMC by a small amount, the production cost of the battery can be reduced while meeting the requirement of improving ion conductivity.
[0045] (3) The present invention can effectively improve the rheological properties of the slurry and the battery preparation process by precisely controlling the ratio of lithium and sodium ions in the binder CMC, thereby helping to reduce the risk of thermal runaway inside the battery and improving battery performance and safety.
[0046] (4) Low lithium content [C6H7O2(OH)2OCH2COONa x Li 1-x ] n It helps to reduce the structural changes of active materials during the cycle process, thereby extending the cycle life of the battery; the solvation energy of sodium ions is lower than that of lithium ions, and the interfacial ion diffusion capacity is better, which helps to improve the fast charging performance of the battery.
[0047] (5) The lithium-rich diaphragm coating binder of the present invention can compensate the lithium ions consumed in the first charge to a certain extent, reduce the exchange reaction of sodium ions with lithium ions ionized from the positive electrode material or the electrolyte, and reduce the efficiency of lithium ion deintercalation in the entire system, thereby alleviating the lithium precipitation phenomenon. The use of lithium-rich diaphragm coating binder can also help shorten the movement path of lithium ions in the battery and improve the performance of the battery.
[0048] The present invention has been described in detail above, but the above embodiments are only illustrative in nature and are not intended to limit the present invention. In addition, this article is not limited by any theory described in the above prior art or invention content or the following examples. DETAILED DESCRIPTION
[0049] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0050] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0051] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, methods in the art.
[0052] Preparation Example Preparation of Catalyst
[0053] Add 54.732g of zirconium oxide, 27.782g of lanthanum powder, and 12.71g of copper powder into a ball mill and mill for 24 hours at a speed of 500rpm to ensure uniform mixing; sinter the uniformly mixed raw materials at a high temperature of 800°C for 5 hours, and then reduce them in a hydrogen atmosphere for 2 hours to obtain a new catalyst 0.6ZrO2·0.2La·0.2Cu.
[0054] Example 1
[0055] 100 g of crushed refined cotton (commercially available, Hunan Sentai Biotechnology Co., Ltd.) was placed in a reactor containing 100 ml of 75 wt% isopropanol-25 wt% tert-butyl alcohol solvent, and 428 ml of 35% NaOH aqueous solution was added, and the reaction was carried out at room temperature 25°C for 60 min; then 300 ml of 50% chloroacetic acid aqueous solution was added and the reaction was carried out at 25°C for 30 min, and the temperature was raised to 55°C and the reaction was carried out for 60 min; the temperature was lowered to room temperature, and hydrochloric acid was added, and the H + The solid was neutralized with OH- in the solution, the solvent and impurities were filtered out, the remaining solid was washed with ethanol for 5 times, and then dried and crushed to obtain CMC-Na powder with a purity of 99.9% and a sodium ion molar mass of 30%.
[0056] CMC-Na and lithium hydroxide were mixed in a sodium-lithium molar ratio of 3:1 in each repeating unit. 242.16 g of CMC-Na was weighed, 2.4 g of lithium hydroxide was added, and 700 ml of water was added as a solvent to form a reaction mixture. Then, the catalyst of the above-mentioned preparation example was added, and the total molar amount of lanthanum powder and copper powder in the catalyst was the same as the molar amount of lithium. The reaction mixture was placed at a constant temperature of 80°C and reacted for 6 hours. After the reaction was completed, an aqueous NaOH solution was added, and [C6H7O2(OH)2OCH2COONa was obtained by filtering, washing, and drying. 0.75 Li 0.25 ] n .
[0057] Example 2
[0058] The same steps as in Example 1 were performed, CMC-Na and lithium hydroxide were mixed according to the sodium-lithium molar ratio of 3.54:1 in each repeating unit to prepare [C6H7O2(OH)2)CH2COONa 0.78 Li 0.22 ] n .
[0059] Example 3
[0060] The steps are the same as those in Example 1. CMC-Na and lithium hydroxide are mixed at a sodium-to-lithium molar ratio of 4:1 in each repeating unit to prepare [C6H7O2(OH)2OCH2COONa 0.8 Li 0.2 ] n .
[0061] Comparative Example 1
[0062] The steps are the same as those in Example 1. CMC-Na and lithium hydroxide are mixed in a sodium-to-lithium molar ratio of 1:3 in each repeating unit to prepare [C6H7O2(OH)2OCH2COONa 0.25 Li 0.75 ] n .
[0063] Comparative Example 2
[0064] The same steps as in Example 1 were performed, CMC-Na and lithium hydroxide were mixed in a sodium-lithium molar ratio of 1:2 in each repeating unit to prepare [C6H7O2(OH)2OCH2COONa 0.33 Li 0.67 ] n .
[0065] Comparative Example 3
[0066] The same steps as in Example 1 were performed, CMC-Na and lithium hydroxide were mixed in a sodium-to-lithium molar ratio of 1:1 in each repeating unit to prepare [C6H7O2(OH)2OCH2COONa 0.5 Li 0.5 ] n .
[0067] Comparative Example 4
[0068] The steps are the same as those in Example 1. CMC-Na and lithium hydroxide are mixed in a sodium-to-lithium molar ratio of 2:1 in each repeating unit to prepare [C6H7O2(OH)2OCH2COONa 0.67 Li 0.33 ] n .
[0069] Comparative Example 5
[0070] The same steps as in Example 1 were performed, CMC-Na and lithium hydroxide were mixed at a sodium-lithium molar ratio of 5.67:1 in each repeating unit to prepare [C6H7O2(OH)2OCH2COONa 0.85 Li 0.15 ] n .
[0071] Comparative Example 6
[0072] The same steps as in Example 1 were performed, CMC-Na and lithium hydroxide were mixed in a sodium-to-lithium molar ratio of 9:1 in each repeating unit to prepare [C6H7O2(OH)2OCH2COONa 0.9 Li 0.1 ] n .
[0073] The binders obtained in the examples and comparative examples were used to prepare diaphragms according to the following method:
[0074] S1: Take 4 parts by weight of the obtained [C6H7O2(OH)2OCH2COONa x Li 1-x ] n The mixture was dissolved in 96 parts by weight of ultrapure water to prepare a binder solution with a solid content of 4%. The speed of the high-speed stirrer was set to 800 rpm and the stirring time was set to 4 hours.
[0075] S2: Preparation of slurry: add 50 parts by weight of ultrapure water and 0.5 parts by weight of polycarboxylate (China Federation, K001) in a beaker in sequence, set the high-speed stirrer to 500 rpm, and set the time for 5 min; add 40 parts by weight of alumina, set the high-speed stirrer to 800 rpm, and set the time for 20 min; add 10 parts by weight of the prepared binder solution, set the high-speed stirrer to 800 rpm, and set the time for 10 min; add 5 parts by weight of polyacrylate (Shandong Poly Chemical Co., Ltd., 9003-01-4), set the high-speed stirrer to 500 rpm, and set the time for 10 min; add 0.01 parts by weight of polyether modified polysiloxane (Shanghai Ziyi Chemical Co., Ltd., ZY-2084), set the high-speed stirrer to 500 rpm, and set the time for 5 min.
[0076] S3: Preparation of diaphragm: Use a 30# wire rod to evenly coat the prepared slurry on a polyethylene porous base membrane (thickness 12μm, porosity 45%, average pore size 70nm). The slurry is controlled at room temperature 20-25℃, and the coated diaphragm is placed in a 40℃ oven for 30s to obtain a diaphragm.
[0077] The performance test of the diaphragm obtained in the embodiment and the comparative example:
[0078] The air permeability value is tested according to the method specified in GB / T 1038, and the thermal shrinkage is tested according to the method specified in GB / T12027-2004.
[0079] Internal resistance: The internal resistance test is carried out in accordance with the GB / T 31485-2015 test standard.
[0080] Ionic conductivity: Tested by electrochemical impedance spectroscopy (EIS) on an electrochemical workstation. The diaphragm is sandwiched between two pairs of steel sheets to form a steel sheet / diaphragm / steel sheet structure, and electrolyte is added to assemble a CR2032 button cell. The electrochemical workstation program is set to 0.01Hz-4MHz, 5m AC signal amplitude. The ionic conductivity is calculated using the following formula:
[0081]
[0082] Where σ is the ionic conductivity, L is the thickness of the membrane, Rt is the bulk impedance measured by the membrane, S (cm 2 ) is the effective contact area between the steel sheet and the diaphragm. The interfacial impedance of the battery was tested by the AC impedance of the electrochemical workstation. The battery was assembled into a Li / diaphragm / Li structure, and the program of the electrochemical workstation was set to 0.01Hz-4MHz, 5mV AC signal amplitude.
[0083] Slurry rheology: It is expressed by the slurry viscosity, and the viscosity test is carried out using Brookfield DV2T.
[0084] Peel strength: Refer to GB / T 2790 adhesive 180° peel strength test.
[0085] Bond strength: Tested in accordance with the requirements of GB / T 2792. Stack A4 paper and diaphragm in the order of A4 paper / diaphragm / diaphragm / A4 paper, with the diaphragm coating facing each other; heat-plasticize the stacked A4 paper / diaphragm at 100°C; cut the heat-plasticized diaphragm into strips of 200 mm in length and 25 mm in width, with the distance between the fixtures being 100±5 mm and the test speed being 50±10 mm / min.
[0086] Heat shrinkage: Tested in accordance with the requirements of GB / T12027-2004.
[0087] 1) Cut a diaphragm of 10*10cm in size, and measure the longitudinal and transverse lengths of the sample with a ruler along the longitudinal and transverse directions marked on the surface of the diaphragm;
[0088] 2) Use a ruler to measure the longitudinal and transverse lengths of the sample;
[0089] 3) Place the sample flat in the fixture, then place it in an oven and keep it at 130°C for 60 minutes;
[0090] 4) After heating, take out the sample, wait until it returns to room temperature, measure the longitudinal and transverse mark lengths again, calculate the shrinkage rate according to the following formula, and finally take the average value of several samples as the shrinkage rate.
[0091]
[0092] ΔL——Thermal shrinkage in the longitudinal direction of the specimen, expressed in %;
[0093] L0——The length of the sample in the longitudinal direction before heating, in millimeters (mm);
[0094] L——The length of the sample in the longitudinal direction after heating, in millimeters (mm);
[0095] ΔT——Thermal shrinkage in the transverse direction of the specimen, expressed in %;
[0096] T o ——The transverse length of the sample before heating, in millimeters (mm);
[0097] T is the transverse length of the sample after heating, in millimeters (mm).
[0098] The results are shown in Table 1.
[0099] Table 1
[0100]
[0101]
[0102] From Table 1, we can see that [C6H7O2(OH)2OCH2COONa x Li 1-x ] n Among them, when 0.75≤x≤0.80 is used for Examples 1 / 2 / 3, the comprehensive performance of the diaphragm is the best. When x<0.75 is used for Comparative Examples 1 / 2 / 3 / 4, the peel strength and thermal shrinkage performance of the diaphragm are poor due to the small number of sodium ions. When x>0.8 is used for Comparative Examples 5 / 6, the ionic conductivity is low due to the small number of lithium ions.
[0103] Using a specific sodium-lithium ratio [C6H7O2(OH)2OCH2COONa x Li 1-x ] n(x accounts for 0.75-0.80), which can not only meet the requirements of improving the ionic conductivity of the diaphragm, but also reduce costs. In the energy storage system, it helps to reduce the structural changes of active materials during the cycle process, thereby extending the cycle life of the battery.
[0104] Power-on performance
[0105] The diaphragm provided in the above embodiment is assembled into a button cell: the embodiment diaphragm is assembled into a CR2032 type button cell, the positive electrode material is lithium iron phosphate, the negative electrode material is graphite, and the electrolyte is 1M (mol / L) LiPF6 ethylene carbonate / dimethyl carbonate solution. The operation is carried out in a glove box under a high-purity argon protective atmosphere, and the button cell is assembled in the order of negative electrode shell, lithium sheet, diaphragm, electrolyte, electrode sheet, gasket, spring sheet, and positive electrode shell, and the packaging machine is used for packaging. After packaging, the button cell is placed in the Arbin battery charge and discharge test system for battery performance testing.
[0106] The test steps of the charge rate performance include: charging the battery to 4.2V at a current of 0.1C, then discharging it to 3.0V, recording the charge capacity and discharge capacity, and calculating the charge rate.
[0107] The first charge cycle efficiency test steps include: subjecting the battery to 100 charge and discharge cycles at room temperature, recording the charge capacity and discharge capacity each time, and analyzing the battery cycle performance. First cycle efficiency = discharge capacity / charge capacity × 100%.
[0108] The results are shown in Table 2.
[0109] Table 2
[0110]
[0111] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A lithium ion battery separator coating binder, It is characterized in that The chemical formula of the lithium ion battery separator coating binder is [C 6 H 7 O 2 (OH) 2 OCH 2 COONa x Li 1-x ] n , where 0.75≤x≤0.80, and n is a natural number greater than 0.
2. A method for preparing the lithium ion battery separator coating binder according to claim 1, It is characterized in that The following steps are involved: (1) Provide sodium carboxymethyl cellulose [C 6 H 7 O 2 (OH) 2 OCH 2 COONa] n ; (2) [C 6 H 7 O 2 (OH) 2 OCH 2 COONa] n The method comprises mixing the sodium source with the lithium source according to the sodium to lithium molar ratio of 75:25-80:20 in each repeating unit, adding a solvent to form a reaction mixture; then adding a catalyst to the reaction mixture, and reacting under a constant temperature; after the reaction is completed, adding a precipitant, filtering, washing, and drying to obtain a lithium ion battery separator coating binder [C 6 H 7 O 2 (OH) 2 OCH 2 COONa x Li 1-x ] n , wherein 0.75≤x≤0.80, n is a natural number greater than 0; wherein the catalyst is composed of zirconium oxide, lanthanum powder and copper powder, the molar ratio of zirconium oxide, lanthanum powder and copper powder is 50-70:10-20:20-30, and the total molar amount of lanthanum powder and copper powder is the same as the molar amount of lithium.
3. The preparation method according to claim 2, It is characterized in that The preparation method of sodium carboxymethyl cellulose in step (1) comprises the following steps: a. Alkalization: the crushed refined cotton is put into a reactor filled with isopropanol-tert-butanol solvent, 30-55% sodium hydroxide aqueous solution is added with stirring, and alkalization is carried out at room temperature for 40-120 minutes; the mass ratio of isopropanol and tert-butanol in the isopropanol-tert-butanol solvent is 75:25; b. Etherification: add 50-80% chloroacetic acid aqueous solution, react at 25-30 ° C for 30-40 minutes, heat to 55-60 ° C and react for 50-60 minutes, cool to room temperature; wherein the mass ratio of refined cotton: sodium hydroxide: chloroacetic acid is 20-30:30-40:30-40; c. Purification: After neutralization with hydrochloric acid, filter, wash with ethanol 3-5 times, dry and crush to obtain sodium carboxymethyl cellulose.
4. The preparation method according to claim 2, It is characterized in that In step (2), the lithium source is one or more selected from lithium hydroxide or lithium carbonate.
5. The preparation method according to claim 2, It is characterized in that In step (2), the solvent is water, and the solid-liquid ratio is 100 g: 300-400 mL.
6. The preparation method according to claim 2, It is characterized in that In step (2), the reaction temperature is 75-80°C, the reaction time is 6-7 hours, and the pH is 9-10.
7. A lithium-rich diaphragm, It is characterized in that It comprises a base film and a lithium-rich ceramic coating, wherein the lithium-rich ceramic coating comprises ceramic powder, and the lithium-ion battery diaphragm coating binder according to claim 1 or the lithium-ion battery diaphragm coating binder prepared by the preparation method according to any one of claims 2-6.
8. The lithium-rich separator according to claim 7, It is characterized in that The ceramic powder is at least one selected from silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, calcium oxide, boehmite, aluminum nitride, boron nitride, barium sulfate, calcium fluoride, barium fluoride, and barium titanate.
9. A method for preparing the lithium-rich separator according to claim 7 or 8, It is characterized in that The following steps are involved: (1) dissolving the lithium ion battery separator coating binder in water to prepare a binder solution with a solid content of 3% to 5%; (2) mixing 40 to 60 parts by weight of water, 0.3 to 0.5 parts by weight of a dispersant, 30 to 40 parts by weight of a ceramic powder, 10 to 20 parts by weight of the binder solution, 5 to 10 parts by weight of a polyacrylate, and 0.005 to 0.01 parts by weight of a wetting agent to prepare a slurry; (3) The prepared slurry is coated on the base film and dried to obtain a lithium-rich separator.
10. A battery, It is characterized in that It comprises the lithium-rich diaphragm according to claim 7 or 8 or the lithium-rich diaphragm prepared by the preparation method according to claim 9.