Coating transfer diaphragm as well as preparation method and application thereof

By regulating the adhesive relationship of the composite coating, ensuring that it remains on the surface of the positive electrode sheet at high temperatures, the short circuit problem caused by thermal shrinkage of the diaphragm is solved, and the safety and performance of the secondary battery are improved.

CN119009357APending Publication Date: 2024-11-22SVOLT ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411285986.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing diaphragm heat shrinkage at high temperatures causes contact between the positive and negative electrodes of the secondary battery, causing the risk of short circuits, and the uniformity and adhesion of the water-based coating are reduced, which cannot effectively prevent short circuits.

Method used

A composite coating structure is adopted, wherein the dry adhesive force between the first coating and the substrate is regulated to F1, and the dry adhesive force between the second coating and the positive electrode sheet is regulated to F2, so that F2/F1≥ 1.0, ensure that the composite coating is completely transferred to the surface of the positive electrode sheet after hot pressing and remains intact after the electrolyte is wet, reducing the risk of short circuit.

Benefits of technology

It improves the adhesive force and ionic conductivity of the diaphragm, reduces the risk of short circuit and fire in the secondary battery, and enhances the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043121900000131
    Figure BDA0005043121900000131
  • Figure BDA0005043121900000141
    Figure BDA0005043121900000141
  • Figure BDA0005043121900000151
    Figure BDA0005043121900000151
Patent Text Reader

Abstract

The invention provides a coating transfer diaphragm as well as a preparation method and application thereof. The coating transfer diaphragm comprises a base material and a composite coating arranged on at least one side of the base material, the composite coating comprises a first coating and a second coating arranged on the surface of the first coating, and the composite coating can be transferred to the surface of a positive plate after being pressed; the dry bonding force between the first coating and the base material is F1, the dry bonding force between the second coating and the positive plate is F2, and the relational expression between F1 and F2 meets the condition that F2 / F1 is greater than or equal to 1.0. The coating transfer diaphragm provided by the invention not only has good adhesive force, but also the contained second oil coating can be completely transferred to the surface of the positive plate and can still be completely retained on the surface of the positive plate after being infiltrated by electrolyte, so that the short-circuit risk of the secondary battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of diaphragm materials, and in particular relates to a coating transfer diaphragm and a preparation method and application thereof. Background Art

[0002] With the rapid development of secondary battery technology, the safety characteristics of secondary batteries have received increasing attention. Among them, battery short circuit is one of the important reasons for battery failure, fire and even explosion. As one of the important components of secondary batteries, the diaphragm not only prevents the positive and negative electrodes inside the battery from directly contacting each other, thereby avoiding the occurrence of short circuits, but also allows ions to move between the positive and negative electrodes to realize the battery's charging and discharging process. At the same time, the material, porosity and thermal stability of the diaphragm have a direct impact on the electrochemical performance and safety of secondary batteries.

[0003] At present, since the main raw materials of the base film in the diaphragm are polyethylene or polypropylene, the heat deformation temperature of the above-mentioned polyolefin material is low. When the temperature is too high, the base film is easy to shrink, which eventually causes the diaphragm to shrink severely, inducing a short circuit in the contact between the positive and negative electrodes in the secondary battery, and then causing thermal runaway of the secondary battery. In order to solve the above problems, researchers usually apply a layer of high-temperature resistant coating material on the surface of the diaphragm, which can improve the thermal shrinkage performance of the diaphragm, and at the same time increase the puncture strength of the diaphragm to prevent lithium dendrites from piercing, thereby improving the safety of the secondary battery. However, although the above-mentioned coated diaphragm disclosed in the prior art can reduce the short-circuit risk of the secondary battery to a certain extent, the coating is mostly water-based. Since the diaphragm itself is lipophilic, water-based coating may cause the uniformity and adhesion of the product to decrease, thereby affecting the quality of the water-based coating and the performance of the battery. In addition, the water-based coating is easy to fall off when wetted by the electrolyte, so the short-circuit risk of the secondary battery is still unavoidable.

[0004] Therefore, in this field, there is an urgent need to develop a diaphragm material to solve the above technical problems. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a coating transfer diaphragm and its preparation method and application. The coating transfer diaphragm provided by the present invention not only has good adhesion, but also the second oil-based coating contained therein can be completely transferred to the surface of the positive electrode sheet and can still be completely retained on the surface of the positive electrode sheet after being infiltrated by the electrolyte, thereby improving the short circuit risk of the secondary battery.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a coating transfer diaphragm, the coating transfer diaphragm comprising a substrate and a composite coating disposed on at least one side of the substrate, the composite coating comprising a first coating and a second coating disposed on the surface of the first coating, the composite coating being capable of being transferred to the surface of a positive electrode sheet after a pressing process;

[0008] The dry bonding strength between the first coating and the substrate is F 1 The dry bonding strength between the second coating and the positive electrode sheet is F 2 , the F 1 With F 2 The relationship between them satisfies: F 2 / F 1 ≥1.0, for example, it can be 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 2, 3, 4, 5, 6, 7, 8, 9, etc.

[0009] It should be noted that the dry adhesive strength refers to the adhesive strength obtained in a dry state, that is, without using a liquid medium. The test conditions of the dry adhesive strength include testing according to GB / T363363-2018 standard. In addition, the first coating is disposed on the surface of at least one side of the substrate, and the second coating is disposed on the surface of the first coating away from the substrate.

[0010] The coating transfer diaphragm provided by the present invention has good adhesion, and further regulates the dry adhesion between the first coating and the substrate and the dry adhesion between the second coating and the positive electrode, so that the adhesion of the second coating is improved, while reducing the adhesion of the first coating, so that the composite coating can be completely transferred to the surface of the positive electrode after hot pressing and the second coating can still be completely retained on the surface of the positive electrode after being soaked in the electrolyte, so that even if the diaphragm shrinks at high temperature, the secondary battery will not be short-circuited due to direct contact between the positive and negative electrodes, thereby improving the safety performance of the secondary battery. Compared with the water-based coating diaphragm disclosed in the prior art, the second oil-based coating provided by the present invention has higher adhesion, and is not easy to fall off after being soaked in the electrolyte, so it can be better attached to the surface of the positive electrode. In addition, the composite coating provided by the present invention has a higher ionic conductivity, which can reduce the injection amount of the electrolyte, thereby reducing the fire risk of the secondary battery.

[0011] Preferably, the F 1 With F 2 The relationship between them satisfies: 1.4≤F 2 / F 1 ≤8.0, for example, it can be 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 7.8, etc.

[0012] In the present invention, by regulating F 1 With F 2 The relationship between enables the composite coating to be transferred to the surface of the positive electrode sheet after hot pressing. After the composite coating is transferred to the surface of the positive electrode sheet, the composite coating can still be maintained on the surface of the positive electrode sheet even when the diaphragm shrinks severely at high temperatures, thereby preventing direct contact and short circuit between the positive and negative electrodes, thereby improving the safety performance of the secondary battery.

[0013] Preferably, the F 1 The value range is 10N / m~30N / m, preferably 15~25N / m, for example, it can be 10N / m, 12N / m, 15N / m, 18N / m, 20N / m, 22N / m, 25N / m, 28N / m, 30N / m, etc.

[0014] Preferably, the F 2 The value range of is 30N / m~80N / m, preferably 35~70N / m, for example, it can be 30N / m, 32N / m, 35N / m, 38N / m, 40N / m, 42N / m, 45N / m, 48N / m, 50N / m, 52N / m, 55N / m, 58N / m, 60N / m, 62N / m, 65N / m, 68N / m, 70N / m, 72N / m, 75N / m, 78N / m, 80N / m and the like.

[0015] Preferably, the thickness of the substrate is H 1 , the thickness of the first coating is H 2 , the thickness of the second coating is H 3 , the H 1 , H 2 With H 3 The relationship between satisfies: 0.7≤H 1 / (H 2 +H 3 )≤10, preferably 1≤H 1 / (H 2 +H 3 )≤8, for example, it can be 0.7, 0.8, 1, 1.2, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, etc.

[0016] In the present invention, by regulating H 1 , H 2 With H 3 The relationship between makes the thermal shrinkage of the coating transfer membrane at high temperature smaller, thereby further improving the safety performance of the secondary battery.

[0017] Preferably, the H 1The value range of is 5 to 20 μm, preferably 5 to 16 μm, for example, it can be 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 16 μm, 18 μm, 20 μm, etc.

[0018] Preferably, the H 2 The value range of is 1 to 4 μm, preferably 1 to 3 μm, for example, it can be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, etc.

[0019] Preferably, the H 3 The value range of is 1 to 3 μm, preferably 1 to 2 μm, for example, it can be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, etc.

[0020] Preferably, the material in the first coating layer includes a semi-solid material, an ion-conducting material and a heat-resistant material.

[0021] Preferably, the mass ratio of the semi-solid material, the ion-conducting material and the heat-resistant material is (2-5):(90-95):(2-5), for example, it can be 2:90:2, 2:91:2, 2:92:3, 3:93:3, 4:94:5, 5:94:5, 2:95:3, 3:94:4, 5:95:5, etc.

[0022] Preferably, the semi-solid material includes at least one of lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide or lithium lanthanum zirconium titanium oxide.

[0023] Preferably, the average particle size of the semi-solid material is 0.5-1.0 μm, for example, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, etc.

[0024] Preferably, the ionic conductivity of the semi-solid material is 10 -3 ~10 -4 S / cm, for example, can be 10 -3 S / cm, 9×10 -4 S / cm, 8×10 -4 S / cm, 7×10 -4 S / cm, 6×10 -4 S / cm, 5×10 -4 S / cm, 4×10 -4 S / cm, 3×10 -4 S / cm, 2×10 -4 S / cm, 1×10 -4 S / cm, etc.

[0025] Preferably, the ion-conducting material comprises molybdenum disulfide and / or a metal organic framework compound.

[0026] In the present invention, the metal organic framework compound illustratively includes at least one of a Zn-based metal organic framework material (MOF), a Ni-based MOF, a Fe-based MOF or a Co-based MOF.

[0027] Preferably, the ionic conductivity of the ion-conducting material is 10 -3 ~10 -4 S / cm, for example, can be 10 -3 S / cm, 9×10 -4 S / cm, 8×10 -4 S / cm, 7×10 -4 S / cm, 6×10 -4 S / cm, 5×10 -4 S / cm, 4×10 -4 S / cm, 3×10 -4 S / cm, 2×10 -4 S / cm, 1×10 -4 S / cm, etc.

[0028] Preferably, the heat-resistant material comprises silicide.

[0029] Preferably, the silicide includes at least one of molybdenum silicide, titanium silicide or nickel silicide.

[0030] Preferably, the average particle size of the heat-resistant material is 0.5-1.8 μm, for example, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm, etc.

[0031] Preferably, the material of the first coating layer further includes a first binder material, and the first binder material exemplarily includes at least one of a polyacrylic acid binder, a polyacrylonitrile binder or a polyacrylamide binder.

[0032] Preferably, the material of the second coating layer includes an oil-based polymer.

[0033] Preferably, the oil-based polymer includes polyolefin microspheres and / or hydrogenated nitrile rubber.

[0034] In the present invention, the material of the substrate is a high temperature resistant substrate material, for example, it may be at least one of aramid or polyimide.

[0035] In a second aspect, the present invention provides a method for preparing the coating transfer membrane according to the first aspect, the method comprising the following steps:

[0036] Mixing the material of the first coating layer and the first solvent to prepare a first coating layer slurry; coating the first coating layer slurry on at least one side of the substrate once, and obtaining the first coating layer after drying;

[0037] The material of the second coating layer is mixed with the second solvent to prepare a second coating layer slurry; the second coating layer slurry is coated on the surface of the first coating layer for a second time, and the coating transfer membrane is obtained after drying.

[0038] Preferably, the first solvent comprises water.

[0039] Preferably, the one-time coating method includes gravure transfer coating.

[0040] Preferably, the surface density of the primary coating is 2.8 to 5.6 g / m 2 , for example, it can be 2.8g / m 2 , 3g / m 2 3.2g / m 2 3.5g / m 2 3.8g / m 2 , 4g / m 2 4.2g / m 2 4.5g / m 2 4.8g / m 2 , 5g / m 2 5.2g / m 2 5.4g / m 2 5.6g / m 2 wait.

[0041] Preferably, the second solvent comprises at least one of N-methylpyrrolidone or N,N-dimethylacetamide.

[0042] Preferably, the secondary coating method includes at least one of roller coating or spray coating.

[0043] Preferably, the surface density of the secondary coating is 0.3-0.5 g / m 2 , for example, it can be 0.3g / m 2 , 0.32g / m 2 , 0.35g / m 2 , 0.38g / m 2 , 0.4g / m 2 , 0.42g / m 2 , 0.45g / m 2 , 0.48g / m 2 , 0.5g / m 2 wait.

[0044] In a third aspect, the present invention provides a secondary battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator comprises the coating transfer separator according to the first aspect.

[0045] In a fourth aspect, the present invention provides a method for preparing the secondary battery according to the third aspect, the method comprising the following steps:

[0046] The positive electrode sheet, the negative electrode sheet and the coating transfer diaphragm are composited and heat-pressed, and the composite coating is in-situ transferred to the surface of the positive electrode sheet by the pressure during the heat-pressing process, and the secondary battery is obtained after injecting the electrolyte.

[0047] Preferably, the composite process includes a thermal composite lamination process.

[0048] Preferably, the process of the thermal composite lamination process includes: firstly bonding the coating transfer diaphragm and the negative electrode sheet by hot roller pressing, and then forming a sandwich structure of upper and lower layers of coating transfer diaphragm covering the negative electrode sheet by slitting; and then laminating the material forming the sandwich structure of upper and lower layers of coating transfer diaphragm covering the negative electrode sheet with the positive electrode to form an electrode group.

[0049] Preferably, the temperature of the hot roller bonding is 70-120°C, for example, it can be 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, etc.; the pressure is 0.3-0.55Mpa, for example, it can be 0.3Mpa, 0.35Mpa, 0.4Mpa, 0.45Mpa, 0.5Mpa, 0.55Mpa, etc.; the efficiency is 30%-90%, for example, it can be 30%, 40%, 50%, 60%, 70%, 80%, 90%, etc.

[0050] Preferably, the slitting temperature is 170-290°C, for example, 170°C, 190°C, 200°C, 220°C, 250°C, 280°C, 290°C, etc.

[0051] Preferably, the temperature of the hot pressing treatment is 90-105°C, for example, 90°C, 92°C, 95°C, 98°C, 100°C, 105°C, etc., and the time is 60s.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] The present invention provides a coating transfer diaphragm, which has good adhesion, and further regulates the dry adhesion between the first coating and the substrate and the dry adhesion between the second coating and the positive electrode, so that the adhesion of the second coating is improved, while reducing the adhesion of the first coating, so that the composite coating can be completely transferred to the surface of the positive electrode after hot pressing and the second coating can still be completely retained on the surface of the positive electrode after being soaked in the electrolyte, so that even if the diaphragm shrinks at high temperature, the secondary battery will not be short-circuited due to direct contact between the positive and negative electrodes, thereby improving the safety performance of the secondary battery. Compared with the water-based coating diaphragm disclosed in the prior art, the second oil-based coating provided by the present invention has higher adhesion, and is not easy to fall off after being soaked in the electrolyte, so it can be better attached to the surface of the positive electrode. In addition, the composite coating provided by the present invention has a higher ionic conductivity, which can reduce the injection amount of the electrolyte, thereby reducing the fire risk of the secondary battery. DETAILED DESCRIPTION

[0054] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0055] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0056] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0057] Example 1

[0058] This embodiment provides a coating transfer diaphragm, which includes an aramid substrate and a composite coating arranged on both sides of the aramid substrate. The composite coating includes a first coating and a second coating arranged on the surface of the first coating. The composite coating can be transferred to the surface of the positive electrode after hot pressing treatment.

[0059] Among them, the dry bonding strength between the first coating and the aramid substrate is F 1 , F 1 The value of is 20N / m; the dry bonding force between the second coating and the positive electrode is F 2 , F 2 The value of F is 55N / m; 1 With F 2 The relationship between them satisfies: F 2 / F 1 =2.75. The thickness of the aramid substrate is H 1 , H 1 The value of is 12μm; the thickness of the first coating is H 2 , H 2The value of is 2μm; the thickness of the second coating is H 3 , H 3 The value of H is 2μm; 1 , H 2 With H 3 The relationship between them satisfies: 1 / (H 2 +H 3 )=3.

[0060] This embodiment also provides a method for preparing the above-mentioned coating transfer membrane, and the preparation method comprises the following steps:

[0061] The mass ratio of lithium aluminum titanium phosphate (average particle size 0.7 μm, ion conductivity 1.3×10 -4 S / cm), molybdenum disulfide (ionic conductivity is 1.1×10 -4 S / cm) and flaky molybdenum silicide (average particle size of 1.1 μm) were mixed with a polyacrylic acid binder material and water to prepare a first coating slurry; the first coating slurry was coated on both sides of the aramid substrate by gravure transfer coating, and the coating surface density was 4.2 g / m 2 , after drying, a first coating is obtained;

[0062] The polyolefin microspheres with a weight average molecular weight of 50W were mixed with N-methylpyrrolidone solvent to prepare a second coating slurry; the second coating slurry was secondarily roll-coated on the surface of the first coating, and the coating surface density was 0.4g / m 2 , and after drying, the coating transfer membrane is obtained.

[0063] Example 2

[0064] This embodiment provides a coating transfer diaphragm, which includes an aramid substrate and a composite coating arranged on both sides of the aramid substrate. The composite coating includes a first coating and a second coating arranged on the surface of the first coating. The composite coating can be transferred to the surface of the positive electrode after hot pressing treatment.

[0065] Among them, the dry bonding strength between the first coating and the aramid substrate is F 1 , F 1 The value of is 15N / m; the dry bonding force between the second coating and the positive electrode is F 2 , F 2 The value of F is 35N / m; 1 With F 2 The relationship between them satisfies: F 2 / F 1 =2.3. The thickness of the aramid substrate is H 1 , H 1 The value of is 16μm; the thickness of the first coating is H2 , H 2 The value of is 3μm; the thickness of the second coating is H 3 , H 3 The value of H is 1μm; 1 , H 2 With H 3 The relationship between them satisfies: 1 / (H 2 +H 3 )=4.

[0066] This embodiment also provides a method for preparing the above-mentioned coating transfer membrane, and the preparation method comprises the following steps:

[0067] The mass ratio of lithium aluminum titanium phosphate (average particle size 0.6 μm, ion conductivity 1.3×10 -4 S / cm), molybdenum disulfide (ionic conductivity is 1.1×10 -4 S / cm) and flaky molybdenum silicide (average particle size of 0.9 μm) were mixed with a polyacrylic acid binder material and water to prepare a first coating slurry; the first coating slurry was coated on both sides of the aramid substrate by gravure transfer, and the coating surface density was 3.5 g / m 2 , after drying, a first coating is obtained;

[0068] The polyolefin microspheres with a weight average molecular weight of 35W were mixed with N-methylpyrrolidone solvent to prepare a second coating slurry; the second coating slurry was secondarily roll-coated on the surface of the first coating, and the coating surface density was 0.35 g / m 2 , and after drying, the coating transfer membrane is obtained.

[0069] Example 3

[0070] This embodiment provides a coating transfer diaphragm, which includes an aramid substrate and a composite coating arranged on both sides of the aramid substrate. The composite coating includes a first coating and a second coating arranged on the surface of the first coating. The composite coating can be transferred to the surface of the positive electrode after hot pressing treatment.

[0071] Among them, the dry bonding strength between the first coating and the aramid substrate is F 1 , F 1 The value of is 25N / m; the dry bonding force between the second coating and the positive electrode is F 2 , F 2 The value of F is 70N / m; 1 With F 2 The relationship between them satisfies: F 2 / F 1 =2.8. The thickness of the aramid substrate is H 1 , H 1The value of is 7μm; the thickness of the first coating is H 2 , H 2 The value of is 1μm; the thickness of the second coating is H 3 , H 3 The value of H is 2μm; 1 , H 2 With H 3 The relationship between them satisfies: 1 / (H 2 +H 3 )=2.3.

[0072] This embodiment also provides a method for preparing the above-mentioned coating transfer membrane, and the preparation method comprises the following steps:

[0073] The mass ratio of lithium aluminum titanium phosphate (average particle size 0.8 μm, ion conductivity 1.3×10 -4 S / cm), molybdenum disulfide (ionic conductivity is 1.1×10 -4 S / cm) and flaky molybdenum silicide (average particle size of 1.2 μm) were mixed with a polyacrylic acid binder material and water to prepare a first coating slurry; the first coating slurry was coated on both sides of the aramid substrate by gravure transfer coating, and the coating surface density was 4.9 g / m 2 , after drying, a first coating is obtained;

[0074] The polyolefin microspheres with a weight average molecular weight of 65W were mixed with N-methylpyrrolidone solvent to prepare a second coating slurry; the second coating slurry was secondarily roll-coated on the surface of the first coating, and the coating surface density was 0.45 g / m 2 , and after drying, the coating transfer membrane is obtained.

[0075] Example 4

[0076] This embodiment provides a coating transfer diaphragm, which includes an aramid substrate and a composite coating arranged on both sides of the aramid substrate. The composite coating includes a first coating and a second coating arranged on the surface of the first coating. The composite coating can be transferred to the surface of the positive electrode after hot pressing treatment.

[0077] Among them, the dry bonding strength between the first coating and the aramid substrate is F 1 , F 1 The value of is 10N / m; the dry bonding force between the second coating and the positive electrode is F 2 , F 2 The value of F is 30N / m; 1 With F 2 The relationship between them satisfies: F 2 / F 1 =3. The thickness of the aramid substrate is H1 , H 1 The value of is 5μm; the thickness of the first coating is H 2 , H 2 The value of is 1μm; the thickness of the second coating is H 3 , H 3 The value of H is 1μm; 1 , H 2 With H 3 The relationship between them satisfies: 1 / (H 2 +H 3 )=2.5.

[0078] This embodiment also provides a method for preparing the above-mentioned coating transfer membrane, and the preparation method comprises the following steps:

[0079] The mass ratio of lithium lanthanum zirconium oxide (average particle size 0.5 μm, ion conductivity 1×10 -4 S / cm), molybdenum disulfide (ionic conductivity is 1×10 -4 S / cm) and cubic nickel silicide (average particle size of 0.5 μm) were mixed with polyacrylic acid binder material and water to prepare a first coating slurry; the first coating slurry was coated on both sides of the aramid substrate by gravure transfer, and the coating surface density was 3.0 g / m 2 , after drying, a first coating is obtained;

[0080] A hydrogenated nitrile rubber with a weight average molecular weight of 20W was mixed with N-methylpyrrolidone solvent to prepare a second coating slurry; the second coating slurry was secondarily roll-coated on the surface of the first coating, and the coating surface density was 0.3 g / m 2 , and after drying, the coating transfer membrane is obtained.

[0081] Example 5

[0082] This embodiment provides a coating transfer diaphragm, which includes an aramid substrate and a composite coating arranged on both sides of the aramid substrate. The composite coating includes a first coating and a second coating arranged on the surface of the first coating. The composite coating can be transferred to the surface of the positive electrode after hot pressing treatment.

[0083] Among them, the dry bonding strength between the first coating and the aramid substrate is F 1 , F 1 The value of is 30N / m; the dry bonding force between the second coating and the positive electrode is F 2 , F 2 The value of F is 80N / m; 1 With F 2 The relationship between them satisfies: F 2 / F 1=2.67. The thickness of the aramid substrate is H 1 , H 1 The value of is 20μm; the thickness of the first coating is H 2 , H 2 The value of is 4μm; the thickness of the second coating is H 3 , H 3 The value of H is 3μm; 1 , H 2 With H 3 The relationship between them satisfies: 1 / (H 2 +H 3 )=2.86.

[0084] This embodiment also provides a method for preparing the above-mentioned coating transfer membrane, and the preparation method comprises the following steps:

[0085] The mass ratio of lithium lanthanum zirconium oxide was 5:95:5 (average particle size 1.0 μm, ion conductivity 1×10 -3 S / cm), molybdenum disulfide (ionic conductivity is 1×10 -3 S / cm) and cubic nickel silicide (average particle size of 1.8 μm) were mixed with polyacrylic acid binder material and water to prepare a first coating slurry; the first coating slurry was coated on both sides of the aramid substrate by gravure transfer, and the coating surface density was 5.6 g / m 2 , after drying, a first coating is obtained;

[0086] A hydrogenated nitrile rubber with a weight average molecular weight of 60W was mixed with N-methylpyrrolidone solvent to prepare a second coating slurry; the second coating slurry was secondarily roll-coated on the surface of the first coating, and the coating surface density was 0.5 g / m 2 , and after drying, the coating transfer membrane is obtained.

[0087] Example 6

[0088] The difference between this embodiment and embodiment 1 is that the dry bonding strength between the first coating and the aramid substrate is F 1 , F 1 The value of is 20N / m; the dry bonding force between the second coating and the positive electrode is F 2 , F 2 The value of F is 30N / m; 1 With F 2 The relationship between them satisfies: F 2 / F 1 =1.5, and the rest are the same as in Example 1.

[0089] Example 7

[0090] The difference between this embodiment and embodiment 1 is that the dry bonding strength between the first coating and the aramid substrate is F 1 , F 1 The value of is 10N / m; the dry bonding force between the second coating and the positive electrode is F 2 , F 2 The value of F is 100N / m; 1 With F 2 The relationship between them satisfies: F 2 / F 1 =10.0, and the rest are the same as in Example 1.

[0091] Example 8

[0092] The difference between this embodiment and embodiment 1 is that H 1 10μm, H 2 10μm, H 3 10μm, H 1 , H 2 With H 3 The relationship between them satisfies: 1 / (H 2 +H 3 )=0.5, and the rest are the same as those in Example 1.

[0093] Example 9

[0094] The difference between this embodiment and embodiment 1 is that H 1 15μm, H 2 0.5μm, H 3 0.5μm, H 1 , H 2 With H 3 The relationship between them satisfies: 1 / (H 2 +H 3 )=15, and the rest are the same as in Example 1.

[0095] Example 10

[0096] The difference between this embodiment and embodiment 1 is that molybdenum silicide is not added to the first coating, and the rest is the same as embodiment 1.

[0097] Embodiment 11

[0098] The difference between this embodiment and embodiment 1 is that the polyolefin microspheres in the second coating are replaced with polyacrylic acid of equal mass, and the rest are the same as embodiment 1.

[0099] Comparative Example 1

[0100] The difference between this comparative example and Example 1 is that the coating transfer diaphragm is not provided with the first coating layer, and the rest is the same as Example 1.

[0101] Comparative Example 2

[0102] The difference between this comparative example and Example 1 is that the coating transfer diaphragm is not provided with a second coating layer, and the rest is the same as Example 1.

[0103] Comparative Example 3

[0104] The difference between this comparative example and Example 1 is that the dry bonding strength between the first coating and the aramid substrate is F 1 , F 1 The value of is 20N / m; the dry bonding force between the second coating and the positive electrode is F 2 , F 2 The value of F is 10N / m; 1 With F 2 The relationship between them satisfies: F 2 / F 1 =0.5, and the rest are the same as in Example 1.

[0105] Test conditions

[0106] The coating transfer membranes provided in Example 1 and the prior art were assembled into lithium-ion batteries and performance tests were performed. The test method was as follows:

[0107] The coating transfer diaphragm provided in Example 1 and the prior art is compounded with the negative electrode sheet into a continuous coating transfer diaphragm-negative electrode sheet-coating transfer diaphragm sandwich structure composite sheet by hot roller hot pressing, and then the continuous composite sheet is cut into independent composite units by a hot cutter, wherein the composite temperature is 95°C, the composite pressure is 45Mpa, the composite efficiency is 60%, and the hot cutter temperature is 230°C. Finally, the composite unit and the positive electrode sheet are stacked into a pole group by lamination and then hot pressed at 100°C. After the pole group is hot pressed, the pole group is disassembled to observe the transfer of the composite coating to the surface of the positive electrode sheet. After taking a pole group and soaking it in the electrolyte for 24 hours, the pole group is disassembled to observe the transfer of the coating on the surface of the positive electrode sheet. At the same time, the water-based glue layer diaphragm with the same structure in the prior art is used for comparison and verification. The test results are shown in Table 1:

[0108] Table 1

[0109]

[0110]

[0111] It can be seen from Table 1 that the coatings shown by the water-based coating transfer membrane used in the prior art and the oil-based coating transfer membrane provided by the present invention can be completely transferred to the surface of the positive electrode sheet after hot pressing treatment, but after the battery electrode group is immersed in the electrolyte for 24 hours, only the second coating of the oil-based coating transfer membrane provided by the present invention can be completely retained on the surface of the positive electrode sheet, and the water-based membrane coating cannot be obviously observed on the surface of the positive electrode sheet, which further indicates that the wet adhesion effect of the oil-based coating transfer membrane provided by the present invention is better than that of the water-based coating membrane, and meets the transfer requirements.

[0112] The lithium-ion battery obtained after hot pressing was placed in an oven for high-temperature baking test. After baking, the battery short circuit was tested first, and then the battery was disassembled to check the shrinkage of the diaphragm. At the same time, the water-based coating transfer diaphragm battery was used for comparison and verification. The test results are shown in Table 2:

[0113] Table 2

[0114]

[0115] It can be seen from Table 2 that after baking at high temperatures of 150°C, 180°C and 200°C for 1h respectively, the water-based coating transfer diaphragm used in the prior art has severe thermal shrinkage, while the oil-based coating transfer diaphragm provided by the present invention has only slight shrinkage, and the oil-based transfer diaphragm coating can still be completely retained on the surface of the positive electrode after being wetted by the electrolyte, so the lithium-ion battery does not short-circuit, further indicating that the oil-based coating transfer diaphragm provided by the present invention has better safety characteristics than the water-based coating transfer diaphragm.

[0116] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A coating transfer membrane, characterized in that: The coating transfer diaphragm comprises a substrate and a composite coating disposed on at least one side of the substrate, wherein the composite coating comprises a first coating and a second coating disposed on the surface of the first coating, and the composite coating can be transferred to the surface of the positive electrode sheet after a pressing process; The dry bonding strength between the first coating and the substrate is F1, the dry bonding strength between the second coating and the positive electrode sheet is F2, and the relationship between F1 and F2 satisfies: F2 / F1≥1.

0.

2. The coating transfer membrane according to claim 1, characterized in that: The relationship between F1 and F2 satisfies: 1.4≤F2 / F1≤8.0; Preferably, the value range of F1 is 10N / m to 30N / m, preferably 15 to 25N / m; Preferably, the value range of F2 is 30N / m to 80N / m, preferably 35 to 70N / m.

3. The coating transfer membrane according to claim 1 or 2, characterized in that: The thickness of the substrate is H1, the thickness of the first coating is H2, the thickness of the second coating is H3, and the relationship between H1, H2 and H3 satisfies: 0.7≤H1 / (H2+H3)≤10, preferably 1≤H1 / (H2+H3)≤8; Preferably, the value range of H1 is 5 to 20 μm, preferably 5 to 16 μm; Preferably, the value range of H2 is 1 to 4 μm, preferably 1 to 3 μm; Preferably, the value range of H3 is 1 to 3 μm, preferably 1 to 2 μm.

4. The coating transfer membrane according to any one of claims 1 to 3, characterized in that: The materials in the first coating layer include semi-solid material, ion-conducting material and heat-resistant material; Preferably, the mass ratio of the semi-solid material, the ion-conducting material and the heat-resistant material is (2-5):(90-95):(2-5); Preferably, the semi-solid material comprises at least one of lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide or lithium lanthanum zirconium titanium oxide; Preferably, the average particle size of the semi-solid material is 0.5 to 1.0 μm; Preferably, the ionic conductivity of the semi-solid material is 10 -3 ~10 -4 S / cm; Preferably, the ion-conducting material comprises molybdenum disulfide and / or a metal organic framework compound; Preferably, the ionic conductivity of the ion-conducting material is 10 -3 ~10 -4 S / cm; Preferably, the heat-resistant material comprises silicide; Preferably, the silicide includes at least one of molybdenum silicide, titanium silicide or nickel silicide; Preferably, the average particle size of the heat-resistant material is 0.5 to 1.8 μm; Preferably, the material of the first coating layer also includes a first binder material.

5. The coating transfer membrane according to any one of claims 1 to 4, characterized in that: The material of the second coating layer includes an oil-based polymer; Preferably, the oil-based polymer includes polyolefin microspheres and / or hydrogenated nitrile rubber.

6. A method for preparing a coating transfer membrane according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: Mixing the material of the first coating layer and the first solvent to prepare a first coating layer slurry; coating the first coating layer slurry on at least one side of the substrate once, and obtaining the first coating layer after drying; The material of the second coating layer is mixed with the second solvent to prepare a second coating layer slurry; the second coating layer slurry is coated on the surface of the first coating layer for a second time, and the coating transfer membrane is obtained after drying.

7. The method according to claim 6, characterized in that The first solvent includes water; Preferably, the one-time coating method includes gravure transfer coating; Preferably, the surface density of the first coating is 2.8 to 5.6 g / m 2 ; Preferably, the second solvent comprises at least one of N-methylpyrrolidone or N,N-dimethylacetamide; Preferably, the secondary coating method includes at least one of roller coating or spray coating; Preferably, the surface density of the secondary coating is 0.3-0.5 g / m 2 .

8. A secondary battery, characterized in that: The secondary battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, and the separator comprises the coating transfer separator according to any one of claims 1 to 5.

9. A method for preparing a secondary battery according to claim 8, characterized in that: The method comprises the following steps: The positive electrode sheet, the negative electrode sheet and the coating transfer diaphragm are composited and heat-pressed, and the composite coating is in-situ transferred to the surface of the positive electrode sheet by the pressure during the heat-pressing process, and the secondary battery is obtained after injecting the electrolyte.

10. The method according to claim 9, characterized in that The composite process includes a thermal composite lamination process; Preferably, the process of the thermal composite lamination process includes: firstly bonding the coating transfer diaphragm and the negative electrode sheet by hot roller pressing, and then forming a sandwich structure of upper and lower layers of coating transfer diaphragm covering the negative electrode sheet by slitting; and then laminating the material forming the sandwich structure of upper and lower layers of coating transfer diaphragm covering the negative electrode sheet with the positive electrode sheet to form an electrode group; Preferably, the temperature of the hot roller bonding is 70-120°C, the pressure is 0.3-0.55Mpa, and the efficiency is 30%-90%; Preferably, the slitting temperature is 170-290°C; Preferably, the temperature of the hot pressing treatment is 90-105° C. and the time is 60 seconds.

Citation Information

Patent Citations

  • Composite diaphragm, preparation method thereof and secondary battery

    CN115732857A

  • Method for manufacturing an electrochemical cell, electrochemical cell, electrolysis cell device and fuel cell device

    DE102023206560A1

Cited By

  • Aramid diaphragm

    CN121149617A

  • Coating transfer diaphragm, coating roller and battery

    CN121748713A

  • Diaphragm and preparation method and application thereof

    CN122051578A

  • Coating-transfer separator, and preparation method therefor and use thereof

    WO2026057084A1