Bonding resin for composite pipeline as well as preparation method and application of bonding resin
The bonding resin for composite pipelines prepared by using maleic anhydride grafted ethylene/ester copolymer and ethylene/ester/carbon monoxide terpolymer, the bonding problem between POK and polyethylene is solved, and efficient POK is achieved The preparation of /polyethylene composite pipes improves the performance and cost-effectiveness of composite pipes.
Patent Information
- Application Number
- CN202411101717.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
AI Technical Summary
POK's application in the pipeline field is limited by the lack of composite bonding resin with polyethylene, a general-purpose pipe raw material, which limits its application as a core tube of composite pipe.
The bonding resin for composite pipelines consisting of maleic anhydride grafted ethylene/ester copolymer, ethylene/ester/carbon monoxide terpolymer, polyethylene and phase conditioning resin is prepared through a twin screw extrusion mechanism, combined with the combination of Extrusion technology to improve bonding and compatibility.
It achieves good bonding effect between POK and polyethylene, improves the adhesion to the reinforcement, improves the peel strength and shear strength of the composite tube, and is suitable for the preparation of POK/polyethylene composite tubes, reducing costs.
Smart Images

Figure BDA0004989537770000062 
Figure BDA0004989537770000082 
Figure BDA0004989537770000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to an adhesive resin for composite pipes and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] POKETONE (POK for short) is an aliphatic polyketone. It is a high molecular polymer obtained by alternating copolymerization of carbon monoxide olefins, ethylene, propylene and other olefinic unsaturated hydrocarbons. It can be used as general plastics, engineering plastics, special engineering plastics, fibers and films. As a new type of engineering plastic with extremely excellent comprehensive performance, POK is 14 times more wear-resistant than POM, resistant to medium acid and alkali, various fuels, and various chemical solvents. Its impact resistance is 2.3 times that of PBT. It has extremely high barrier properties to water vapor and various hydrocarbons, equivalent to EVOH, and 1.3 times the hydrolysis resistance of PP0. Typical application areas include packaging bottles, automotive parts, pipe lining applications, and industrial filters. In the field of pipelines, POK has become the preferred material for oil production line pipes with its advantages of high temperature resistance, oil resistance, wear resistance, and corrosion resistance. For example: Patent No. CN108297370A discloses a method for making a POK liner tube, including the following steps: S1, making a polyketone liner tube substrate by a screw extruder; S2, compressing the outer diameter of the polyketone liner tube substrate from a first size to a second size by an isodiameter compressor to obtain a polyketone liner tube semi-finished product; S3, inserting the polyketone liner tube semi-finished product into an outer tube; and S4, heating the polyketone liner tube semi-finished product so that the outer wall of the polyketone liner tube semi-finished product is close to the inner wall of the outer tube to obtain a polyketone sleeve. Since the liner tube is made of polyketone material, the long-term safe use temperature of the obtained polyketone sleeve is 120°C, which will not cause the liner tube to fall off and bulge, leading to accidents. Patent No. CN107940123A discloses a polyketone lined oil pipe. The polyketone material, antioxidant and plasticizer are melted and extruded, cooled, and the polyketone lined pipe is obtained; then the polyketone lined pipe is pulled into the oil pipe; finally, both ends of the polyketone lined pipe are heated and softened, and then flanged and trimmed.
[0004] At present, the application of POK in the pipeline field is mainly as the inner lining of oil casing, and the composite method is to insert POK into the inner wall of steel pipe. Although POK has excellent comprehensive performance as a pipeline, the lack of composite adhesive resin between POK and polyethylene, a common pipe raw material, limits the application of POK as the core pipe of composite pipe by co-extrusion of a thin layer. Summary of the invention
[0005] In order to overcome the above problems, the present invention provides an adhesive resin for composite pipes and a preparation method and application thereof.
[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention provides a bonding resin for composite pipes, wherein the raw materials include, by weight: 20 to 40 parts of maleic anhydride grafted ethylene / ester copolymer, 25 to 50 parts of ethylene / ester / carbon monoxide terpolymer, 25 to 40 parts of polyethylene, 3 to 10 parts of phase regulating resin and 0.5 to 1 part of auxiliary agent;
[0008] The maleic anhydride grafted ethylene / ester copolymer is composed of the following raw materials in parts by weight: 100 parts of ethylene / ester copolymer, 1.0-3.0 parts of maleic anhydride and 0.02-0.10 parts of initiator.
[0009] In one or more embodiments, the method for preparing the maleic anhydride grafted ethylene / ester copolymer comprises:
[0010] Ethylene-ester copolymer, maleic anhydride and initiator are uniformly mixed according to the proportion, and the mixed raw materials are extruded through a twin-screw extruder to obtain maleic anhydride grafted ethylene / ester copolymer.
[0011] Preferably, the grafting rate of the maleic anhydride grafted ethylene / ester copolymer is 0.5% to 2%.
[0012] Preferably, the extrusion temperature of the extruder is 250-350°C.
[0013] Preferably, the initiator is a peroxide initiator, including one of 2,5-dimethyl-2,5-di(2-ethylhexanoyl peroxide)hexane, di-tert-butyl peroxide diisopropylbenzene, 2,3-dimethyl-2,3-diphenylbutane, Trigonox311, tert-butyl perbenzoate, and tert-amyl perbenzoate.
[0014] In one or more embodiments, the ethylene / ester copolymer in the maleic anhydride grafted ethylene / ester copolymer includes one or more of ethylene / methyl acrylate copolymer, ethylene / butyl acrylate copolymer or ethylene / vinyl acetate copolymer.
[0015] In one or more embodiments, the ethylene content of the ethylene / ester copolymer is 70 to 73%.
[0016] In one or more embodiments, the ethylene / ester / carbon monoxide terpolymer includes one of ethylene / methyl acrylate / carbon monoxide copolymer, ethylene / ethyl acrylate / carbon monoxide copolymer, ethylene / butyl acrylate / carbon monoxide copolymer or ethylene / vinyl acetate / carbon monoxide copolymer.
[0017] In one or more embodiments, in the ethylene / ester / carbon monoxide terpolymer, the ester content is 10% to 30%, and the carbon monoxide content is 5% to 15%.
[0018] In one or more embodiments, the phase regulating resin includes: poly-α-methylstyrene resin, terpene phenolic resin, rosin glycerol ester, hydrogenated rosin glycerol ester, pentaerythritol rosin ester, hydrogenated pentaerythritol rosin ester, rosin modified phenolic resin, styrene block copolymer.
[0019] In one or more embodiments, the auxiliary agent includes an antioxidant, an ultraviolet light stabilizer, a nucleating agent, and a pigment.
[0020] In one or more embodiments, the polyethylene melt has a mass flow rate of 0.2 to 1.4 g / 10 min (190° C., 5 kg weight).
[0021] The second aspect of the present invention provides a method for preparing the above-mentioned adhesive resin for composite pipes, comprising:
[0022] The maleic anhydride grafted ethylene / ester copolymer, ethylene / ester / carbon monoxide terpolymer, phase regulating resin and additives are uniformly mixed according to the proportion, and the mixed raw materials are extruded through a twin-screw extruder to obtain a bonding resin for composite pipes.
[0023] In one or more embodiments, the extrusion temperature of the extruder is 160-200°C.
[0024] A third aspect of the present invention is the use of the above-mentioned bonding resin for composite pipes to bond a POK layer and a polyethylene layer in the composite pipes.
[0025] In one or more embodiments, the composite pipe includes a reinforcement body, and the reinforcement body includes a steel mesh, glass fiber, polyester fiber or aramid fiber.
[0026] The beneficial effects of the present invention are:
[0027] (1) The ethylene / ester / carbon monoxide terpolymer in the adhesive resin for composite pipes has a polyketone structure similar to that of POK, so it has a good bonding effect on POK; at the same time, the ethylene / ester structure in the ethylene / ester / carbon monoxide terpolymer has a certain compatibility with polyethylene, so the ethylene / ester / carbon monoxide terpolymer has a good bonding effect on POK and polyethylene with large differences in polarity.
[0028] (2) By grafting maleic anhydride onto ethylene / ester copolymer, the maleic anhydride grafted ethylene / ester copolymer obtained after grafting modification can not only improve the compatibility of ethylene / ester / carbon monoxide terpolymer and polyethylene copolymer in the adhesive resin, but also improve the adhesion of the adhesive resin to reinforcements such as steel wire and glass fiber.
[0029] (3) By adding phase regulating resin, the compatibility of each component is further improved, the cohesive strength is adjusted, and it has excellent wettability and good adhesion to POK and polyethylene, two polymers with large polarity differences. The 180° peel strength of POK / polyethylene after bonding is greater than 6N / mm, and the peeling state is cohesive failure; the maleic anhydride grafted ethylene / ester copolymer has a maleic anhydride group with high polarity, and the shear strength between the adhesive resin and the steel wire is greater than 13MPa.
[0030] (4) The adhesive resin for composite pipes provided by the present invention has excellent adhesion to POK and polyethylene, two polymers with a large difference in polarity. Through co-extrusion composite technology, it can be applied to POK / polyethylene composite pipes, wire mesh skeleton reinforced POK / polyethylene composite pipes, glass fiber tape reinforced POK / polyethylene composite pipes, polyester fiber reinforced POK / polyethylene composite pipes and aramid fiber reinforced POK / polyethylene composite pipes, etc.; using high-cost and high-performance POK as the core pipe and conventional low-cost polyethylene as the outer layer, it can be applied to the preparation of cost-effective aliphatic polyketone / polyethylene composite pipes through composite application at a relatively low cost. DETAILED DESCRIPTION
[0031] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0032] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0033] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0034] Example 1
[0035] 1.1 Raw material information:
[0036] The ethylene / ester copolymer is ethylene / methyl acrylate: AC 1330, Dow Chemical;
[0037] Ethylene / ester / carbon monoxide terpolymer is an ethylene / vinyl acetate / carbon monoxide copolymer: 4924, Dow Chemical;
[0038] Polyethylene is PE100 pipe-grade high-density polyethylene: PN-049-030-122, Sinopec (Tianjin) Petrochemical Co., Ltd.
[0039] Phase regulating resin: poly-α-methylstyrene resin, M-80, Wuxi Jiasheng Modified Materials Co., Ltd.;
[0040] Additives: Antioxidant 1010, Beijing Jiyi Chemical Co., Ltd.
[0041] 1.2 Preparation of maleic anhydride grafted ethylene / ester copolymer (Mg-1):
[0042] 100 parts of ethylene / methyl acrylate ( AC 1330, Dow Chemical), 1 part of maleic anhydride, and 0.02 part of di-tert-butyl peroxide diisopropylbenzene were uniformly mixed by high-speed stirring, and reactive extrusion was carried out at 250°C using a twin-screw extruder with a screw length-to-diameter ratio of 40:1 and a diameter of 75 mm. Maleic anhydride-grafted Mg-1 was obtained by reactive extrusion grafting. After acid-base titration test, the monomer grafting rate was 0.62%.
[0043] 1.3 Preparation of bonding resin for composite pipes:
[0044] The components were mixed uniformly by a mixer according to the ratio in Table 1, added into a twin-screw extruder, melt-blended at 190° C., and granulated to obtain adhesive resin particles.
[0045] Table 1 Proportions of bonding resin for composite pipes
[0046]
[0047] 1.4 Testing and application of adhesive resin for composite pipes:
[0048] POK / polyethylene sheet composite 180° peel strength and steel wire shear strength test:
[0049] POK (M730, Hyosung Chemical, South Korea) was pressed into a 2.0 mm sheet at 245°C, polyethylene (2480, Qilu Petrochemical) was pressed into a 0.8 mm sheet at 200°C, and the adhesive resin was pressed into a 0.15 mm film at 200°C. The M730 sheet and the polyethylene sheet were first placed on a flat vulcanizer at 210°C for preheating. After the polyethylene was melted, the adhesive resin was bonded to the polyethylene sheet, and then POK was bonded to the adhesive resin film. The POK / adhesive resin / PE composite sheet was compounded at a pressure of 0.5 MPa for 20 seconds, and after cooling, it was cut into 25 mm wide peel test samples. The 180° peel strength was tested at a tensile speed of 100 mm / min. The relevant data are shown in Table 4.
[0050] According to Appendix A of GB / T32439-2015, the adhesive resin and 0.7 mm steel wire were used to prepare specimens for the shear strength test of the adhesive resin and the steel wire. Eight groups of specimens were tested and the average value was calculated. The relevant data are shown in Table 4.
[0051] 3.2 90° peel test of adhesive resin for POK / PE composite pipe:
[0052] On a three-layer co-extrusion composite pipe processing equipment, POK (M730, Hyosung Chemical, South Korea) is used as the core tube, and the adhesive resin and polyethylene (2480, Qilu Petrochemical) of Example 1 are used as the outer layer. The temperatures of the POK and adhesive resin extruders are controlled to be 240°C, and the processing temperature of the outer polyethylene extruder is controlled to be 200°C. A POK / PE composite pipe with a dn of 110×10 mm is obtained by coextrusion. The thickness of the adhesive resin layer is controlled to be 0.5-1.0 mm, the thickness of the core tube POK is controlled to be 3.0-4.0 mm, and the total thickness is 10.0-10.5 mm. The pipe is cut into 25 mm wide peeling test samples along the pipe direction, and the 90° peeling strength is tested at a tensile speed of 100 mm / min. The relevant data are shown in Table 4.
[0053] Example 2
[0054] 2.1 Raw material information:
[0055] Ethylene / ester copolymer is ethylene / butyl acrylate ( AC 3427, Dow Chemical) and ethylene / vinyl acetate copolymer (V6110M, Yangzi Petrochemical-BASF Co., Ltd.);
[0056] The ethylene / ester / carbon monoxide terpolymer is an ethylene / butyl acrylate / carbon monoxide copolymer: HP441, Dow Chemical;
[0057] Polyethylene is PE80 grade pipeline high-density polyethylene: DGDB2480, Shandong Qilu Petrochemical Company;
[0058] Phase regulating resin: terpene phenolic resin: 803L, Arakawa, Japan;
[0059] Additives: Antioxidant 3114, BASF.
[0060] 2.2 Preparation of maleic anhydride grafted ethylene / ester copolymer (Mg-2):
[0061] 50 parts of ethylene / butyl acrylate ( AC 3427, Dow Chemical), 50 parts of ethylene / vinyl acetate copolymer (V6110M, Yangzi Petrochemical-BASF Co., Ltd.), 1.2 parts of maleic anhydride, and 0.03 parts of 2,5-dimethyl-2,5-di(2-ethylhexanoyl peroxide)hexane were uniformly mixed by high-speed stirring, and reactive extrusion was carried out at 280°C using a twin-screw extruder with a screw length-to-diameter ratio of 44:1 and a diameter of 75 mm. Maleic anhydride-grafted Mg-2 was obtained by reactive extrusion grafting. After acid-base titration test, the monomer grafting rate was 0.79%.
[0062] 2.3 Preparation of bonding resin for composite pipes:
[0063] The components were mixed uniformly by a mixer according to the ratio in Table 2, added into a twin-screw extruder, melt-blended at 180° C., and granulated to obtain adhesive resin particles.
[0064] Table 2 Proportions of bonding resin for composite pipes
[0065]
[0066] 2.4 Testing and application of adhesive resin for composite pipes:
[0067] The tests of 180° peel strength and steel wire shear strength of POK / polyethylene sheet composite are the same as those in Example 1.
[0068] 2.53.2 Adhesive resin is used for bonding POK / PE composite pipes reinforced with steel wire mesh skeleton:
[0069] On a multi-layer co-extruded composite steel wire mesh skeleton reinforced composite pipe processing equipment, extrusion grade POK (M730, Korea Hyosung is OK) is used as the core tube, and the adhesive resin of Example 2 is co-extruded at 240°C. Then, 48 0.7mm steel wires are wound on the core tube by left-handed and right-handed winding, and a 1.2-1.5mm adhesive resin layer of Example 2 is extruded on the surface of the steel wire reinforcement layer. Finally, polyethylene (2480, Qilu Petrochemical) is extruded as the outer layer at a temperature of 210°C on the adhesive resin surface. After cooling, a dn110×2.5MPa steel wire mesh skeleton reinforced POK / PE composite pipe is obtained. The prepared composite pipe is cut into 25mm wide peeling test samples along the pipe direction, and the 90° peeling strength is tested at a tensile speed of 100mm / min. The relevant data are shown in Table 4.
[0070] Comparative Example 1
[0071] The information of the raw materials used in Comparison 1 is the same as that in Example 1.
[0072] The specific steps for preparing the adhesive resin for composite pipes are: preparing according to the proportions in Table 3 and the process in Example 1.
[0073] Table 3 Proportions of bonding resin for composite pipes
[0074]
[0075] The testing and application of the adhesive resin for composite pipes prepared in this embodiment are the same as those in Example 1.
[0076] Example 3
[0077] The 180° peel strength of the adhesive resin bonded to the PA / PE composite sheet and the 90° peel strength of the PA / PE composite pipe obtained by the above examples and comparative examples are shown in Table 4:
[0078] Table 4 180° peel strength, wire shear strength of POK / PE composite sheets bonded with adhesive resin and 90° peel strength of POK / PE composite pipes
[0079]
[0080]
[0081]
[0082]
[0083] From the performance data of Examples 1 to 2 and Comparative Example 1 shown in the above table, it can be seen that:
[0084] The 180° peel strength of the bonding of POK / PE sheets in Examples 1 and 2 of the present invention is greater than 6N / mm, the peeling state is cohesive failure, and the shear strength of the bonding resin to the steel wire is greater than 13MPa; the 180° peel strength of the bonding of POK / PE sheets in Comparative Example 1 is less than 6N / mm, and the peeling state is uncertain. This shows that the bonding resin of the present invention has higher peel strength, the peeling state is cohesive failure, and the stability of the peeling force is good.
[0085] By comparing 1A to 1D of Example 1 and Comparative Example 1 to 3A, it can be seen that not adding the phase-adjusting resin will lead to unstable peel strength of the adhesive resin, and the peeling state changes from cohesive failure to either sticking to POK or sticking to PE; by comparing 1A to 1D of Example 1 and Comparative Example 1 to 4B, it can be seen that when the added phase-adjusting resin exceeds 10 parts, the adhesive resin shows that the peel strength of POK / PE drops to less than 6N / mm, mainly because the molecular weight of the phase-adjusting resin is low, and when the added amount exceeds 10 parts, the cohesive strength of the adhesive resin decreases. The adhesive resin for POK / PE composite pipes of the present invention can make the adhesive resin have good adhesion and immersion to POK and PE by introducing 3 to 10 parts of the phase-adjusting resin into the formula, and the state during peeling is cohesive failure, and the force value stability of the peel strength test is good.
[0086] By comparing Example 1B and Comparative Example 3C, it can be seen that when the amount of ethylene added to the adhesive resin is greater than 40 parts, the peel strength of the adhesive resin to POK / PE becomes lower, and the peeling state changes from cohesive failure to partial non-stick POK.
[0087] By comparing Examples 1 and 2 with Comparative Examples 3D and 3E, it can be seen that when the addition amount of ethylene / butyl acrylate / carbon monoxide copolymer is between 25 and 50 parts, the adhesion of the adhesive resin to POK / PE can be maintained at greater than 6 N / mm; when it exceeds 50 parts, the adhesion of the adhesive resin is low due to the high melt index and low cohesive force of the ethylene / butyl acrylate / carbon monoxide copolymer itself; when it is less than 25 parts, the proportion of ethylene / butyl acrylate / carbon monoxide copolymer having a similar structure to POK is reduced, resulting in a deterioration in the adhesion state between the adhesive resin and POK, resulting in a non-stickiness to POK after peeling.
[0088] By comparing Examples 1 and 2 with Comparative Examples 3E and 3F, it can be seen that when the addition amount of the maleic anhydride grafted ethylene / ester copolymer is 20-40 parts, the bonding of the adhesive resin to POK / PE can be maintained at greater than 6N / mm, and the shear strength to the steel wire is greater than 13MPa; when it exceeds 40 parts, the addition of ethylene / butyl acrylate / carbon monoxide copolymer is low, and the bonding of the adhesive resin to POK is poor; when it is less than 20 parts, the bonding effect of the adhesive resin to the steel wire becomes worse, and the shear strength between the adhesive resin and the steel wire becomes lower.
[0089] It can be seen from Examples 1 and 2 of the present invention that the adhesive resin of the present invention has good adhesion to both POK and polyethylene, and can be used not only for the composite of POK / PE plastic pipes, but also for the composite of POK / PE composite pipes such as steel wire mesh skeleton reinforcement.
[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A bonding resin for a composite pipe, characterized in that: The raw material composition includes, by weight: 20 to 40 parts of maleic anhydride grafted ethylene / ester copolymer, 25 to 50 parts of ethylene / ester / carbon monoxide terpolymer, 25 to 40 parts of polyethylene, 3 to 10 parts of phase regulating resin and 0.5 to 1 part of auxiliary agent; The maleic anhydride grafted ethylene / ester copolymer is composed of the following raw materials in parts by weight: 100 parts of ethylene / ester copolymer, 1.0-3.0 parts of maleic anhydride and 0.02-0.10 parts of initiator.
2. The adhesive resin for composite pipe according to claim 1, characterized in that: The preparation method of the maleic anhydride grafted ethylene / ester copolymer comprises: The ethylene-ester copolymer, maleic anhydride and initiator are uniformly mixed according to the ratio, and the mixed raw materials are extruded through a twin-screw extruder to obtain the maleic anhydride grafted ethylene / ester copolymer; Preferably, the grafting rate of the maleic anhydride grafted ethylene / ester copolymer is 0.5% to 2%. Preferably, the extrusion temperature of the extruder is 250 to 350°C; Preferably, the initiator is a peroxide initiator, including one of 2,5-dimethyl-2,5-di(2-ethylhexanoyl peroxide)hexane, di-tert-butyl peroxide diisopropylbenzene, 2,3-dimethyl-2,3-diphenylbutane, Trigonox311, tert-butyl perbenzoate, and tert-amyl perbenzoate.
3. The adhesive resin for composite pipe according to claim 1, characterized in that: The ethylene / ester copolymer in the maleic anhydride grafted ethylene / ester copolymer includes one or more of ethylene / methyl acrylate copolymer, ethylene / butyl acrylate copolymer or ethylene / vinyl acetate copolymer; Alternatively, the ethylene content in the ethylene / ester copolymer is 70 to 73%.
4. The adhesive resin for composite pipe according to claim 1, characterized in that: The ethylene / ester / carbon monoxide terpolymer includes one of ethylene / methyl acrylate / carbon monoxide copolymer, ethylene / ethyl acrylate / carbon monoxide copolymer, ethylene / butyl acrylate / carbon monoxide copolymer or ethylene / vinyl acetate / carbon monoxide copolymer; Alternatively, in the ethylene / ester / carbon monoxide terpolymer, the ester content is 10% to 30%, and the carbon monoxide content is 5% to 15%.
5. The adhesive resin for composite pipe according to claim 1, characterized in that: The phase regulating resin includes: poly-α-methylstyrene resin, terpene phenolic resin, rosin glycerol ester, hydrogenated rosin glycerol ester, pentaerythritol rosin ester, hydrogenated pentaerythritol rosin ester, rosin modified phenolic resin, styrene block copolymer; Alternatively, the auxiliary agent includes an antioxidant, an ultraviolet light stabilizer, a nucleating agent, and a pigment.
6. The adhesive resin for composite pipe according to claim 1, characterized in that: The polyethylene melt has a mass flow rate of 0.2 to 1.4 g / 10 min (190° C., 5 kg weight).
7. The method for preparing the adhesive resin for composite pipes according to any one of claims 1 to 6, characterized in that: include: The maleic anhydride grafted ethylene / ester copolymer, ethylene / ester / carbon monoxide terpolymer, phase regulating resin and additives are uniformly mixed according to the proportion, and the mixed raw materials are extruded through a twin-screw extruder to obtain a bonding resin for composite pipes.
8. The preparation method according to claim 7, characterized in that: The extrusion temperature of the extruder is 160-200°C.
9. Use of the adhesive resin for composite pipes according to any one of claims 1 to 6 and / or the adhesive resin for composite pipes prepared by the preparation method according to any one of claims 7 to 8 in bonding a POK layer and a polyethylene layer in a composite pipe.
10. The use according to claim 9, characterized in that The composite pipe comprises a reinforcement body, and the reinforcement body comprises a steel mesh, glass fiber, polyester fiber or aramid fiber.