Self-sealing rubber material composition of safety tire as well as preparation method and application of self-sealing rubber material composition

Through the combination of modified nano alumina/titanium oxide duplex and zinc stearate/epoxy soybean oil, the performance problems of self-sealing rubber in high and low temperature environments are solved, and the efficient self-sealing rubber is achieved. Stability meets the puncture prevention needs of different seasons and regions.

CN118931429AActive Publication Date: 2024-11-12ZHONGLIE IND (GUANGDONG) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411071409.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Existing self-sealing materials are prone to soften at high temperatures, causing air leakage, and are prone to brittle cracking at low temperatures, making it difficult to meet the demand for tire puncture prevention in different seasons and regions at the same time. The poor dispersion of the filler affects the mechanical properties and thermal stability of the rubber. .

Method used

Modified nano-alumina/titanium oxide biphasic composites are used as fillers, combined with zinc stearate and epoxy soybean oil as heat stabilizers, and diatomaceous earth or bentonite as additives to improve organic-inorganic component compatibility and dispersibility, enhance the mechanical properties and high and low temperature resistance of the glue.

Benefits of technology

It achieves excellent high and low temperature resistance in the range of -45℃~120℃, avoids degumming, flow and brittle cracking of sealant, and improves the self-sealing performance of the glue and driving safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931429A_ABST
    Figure CN118931429A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of tire self-sealing rubber, and particularly discloses a self-sealing rubber material composition of a safety tire as well as a preparation method and application of the self-sealing rubber material composition. The rubber material comprises the following components: a base material, a tackifier, a two-phase filler, a heat stabilizer, an auxiliary agent, a dispersing agent, an anti-aging agent and a coloring agent, the matrix material is mixed rubber of butyl rubber and ethylene propylene diene monomer, the filler is a modified nano aluminum oxide / titanium oxide two-phase compound, the heat stabilizer is a mixture of zinc stearate and epoxidized soybean oil, the tackifier is silane-terminated modified polybutadiene rubber, the assistant is one of diatomite or bentonite, and the dispersant is polyvinyl alcohol. By screening and modifying the components and the filler, the compatibility between organic-inorganic components is improved, the dispersion of the filler in a matrix is promoted, and the mechanical property and thermal stability of the sealant are enhanced, so that the sealant has excellent high and low temperature resistance and also has an effect of enhancing the self-sealing property of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tire self-sealing adhesives, and in particular relates to a self-sealing adhesive composition for a safety tire, a preparation method thereof and an application thereof. Background Art

[0002] Accidents caused by tire damage during driving are increasing day by day, which constantly affects the safety of vehicles and pedestrians. Tire sealant is a preventive method to prevent tire blowouts. A layer of sealant with self-repairing function is applied inside the tire to prevent problems such as air leakage and blowout when the tire is damaged or punctured by sharp objects.

[0003] At present, butyl rubber, thermoplastic elastomer, styrene-butadiene rubber, and halogenated butyl rubber are mainly used as the main materials of self-sealing adhesives, and inorganic materials such as zinc oxide, silicon oxide, and calcium carbonate are used as fillers. Various additives such as antioxidants, plasticizers, tackifiers, antioxidants, coupling agents, etc. are usually poorly compatible with rubber products. In particular, the dispersion of fillers has a great influence on the processing performance of rubber compounds, which is easy to cause poor dispersion and unevenness, thereby affecting the mechanical properties, thermal stability, and self-sealing performance of the rubber compound itself. For example, due to the large temperature difference between the north and the south or between summer and winter, some self-sealing adhesives currently available on the market will soften at high temperatures, causing strong fluidity, which will easily squeeze out when punctured, causing tire leakage, or flow accumulation when the vehicle is running at high speed, causing tire dynamic imbalance; and when punctured by sharp objects at low temperatures, it is easy to crack; it is difficult to simultaneously meet the needs of car owners for tire puncture protection when changing seasons or driving across regions. Therefore, the quality of rubber compound mixing is related to the degree of subsequent processing and the self-sealing performance of the rubber compound. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present application proposes a self-sealing rubber composition for a safety tire, a preparation method thereof, and an application thereof. By modifying the components and fillers, the compatibility between the organic and inorganic components is improved, the dispersion of the fillers in the matrix is ​​promoted, the various components of the rubber used can play a synergistic role, the mechanical properties and high and low temperature resistance of the rubber are enhanced, the rubber cost is lower, and it has better elasticity, strength and self-sealing properties.

[0005] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0006] The first object of the present invention is to provide a self-sealing rubber material for a safety tire, comprising the following components: a base material, a tackifier, an inorganic filler, a heat stabilizer, an additive, a dispersant, an antioxidant, and a colorant. The base material is a mixed rubber of butyl rubber and EPDM rubber, the inorganic filler is a modified nano-alumina / titanium oxide two-phase composite, and the heat stabilizer is a mixture of zinc stearate and epoxidized soybean oil.

[0007] Furthermore, the components are calculated by weight as follows: 58-75 parts of base material, 4.0-6.5 parts of tackifier, 16-25 parts of inorganic filler, 2.3-4.0 parts of heat stabilizer, 3.0-4.5 parts of auxiliary agent, 0.8-2.0 parts of dispersant, 0.2-1.5 parts of antioxidant, and 0.3-1.2 parts of colorant.

[0008] Furthermore, the weight ratio of butyl rubber to EPDM rubber in the base material is 2:3 to 3:2.

[0009] Furthermore, the tackifier is silane-terminated modified polybutadiene rubber.

[0010] Furthermore, the silane-terminated modified polybutadiene rubber is one of Polyvest EP ST-E 60 and Polyvest EP ST-E100 (commercially available), which is a polybutadiene modified by triethoxysilane end-capping.

[0011] Furthermore, the weight ratio of zinc stearate to epoxy soybean oil in the heat stabilizer is 2-5:1-3.

[0012] The composite heat stabilizer is used in combination in the adhesive component of the present application, and the combination of zinc stearate and epoxy soybean oil can enhance the thermal stability of the sealant. At the same time, the use of auxiliary agents such as diatomaceous earth or bentonite can reduce the moisture in the sealant, making the heat stabilizer more stable and / or the free active groups captured by the heat stabilizer more stable, further enhancing the thermal stability of the sealant, so that the sealant has excellent high and low temperature resistance.

[0013] Furthermore, the inorganic filler modified nano alumina / titanium oxide dual-phase composite is prepared by the following method: modifying nano alumina with polyvinyl pyrrolidone and sodium alginate as surface treatment agents, and then dispersing the nano alumina in toluene to obtain a toluene dispersion of the nano alumina; mixing acetic acid and triethanolamine, adding tetrabutyl titanate and stirring to obtain a mixed solution, then adding the toluene dispersion of the nano alumina to the mixed solution, continuing to stir to obtain a sol, aging and drying the sol, and then grinding to obtain the obtained product.

[0014] The present application adopts a two-phase composite structure of modified alumina / titanium oxide, and uses polyvinyl pyrrolidone and sodium alginate as surface treatment agents to modify the alumina, thereby improving the interaction effect between the base material and the inorganic phase, and interacting with the active sites in the matrix, further improving the high and low temperature resistance. At high temperatures, the rubber is stable, and the sealant and the tire airtight layer have a high adhesion retention rate. At low temperatures, the brittleness and crack resistance of the sealant are reduced, so that the self-sealing performance of the resulting rubber is effectively improved.

[0015] The presence of titanium oxide in the modified alumina / titania dual-phase system prepared in the present application effectively reduces the interaction between alumina particles and promotes the dispersion of fillers in the matrix. Compared with the rubber composite material with direct addition of alumina / titania, the dual-phase filler has a lower degree of filler networking and a more uniform dispersion of the filler, thereby significantly improving the elongation at break and tensile strength, and can improve the thixotropy and heat resistance of the rubber, reduce the difference in thermal expansion coefficient between the sealant and the joint surface, and also have a significant enhancing effect on the sealing effect of the material.

[0016] Furthermore, in a specific embodiment of the present invention, the modified nano-alumina / titanium oxide dual-phase composite is prepared by the following specific steps:

[0017] 30-50 parts of nano-alumina and 1.5-4.2 parts of modifiers polyvinyl pyrrolidone and sodium alginate are added to 80-150 parts of aqueous solution, the mass ratio of polyvinyl pyrrolidone to sodium alginate is 3-5:1, ultrasonic treatment is performed for 15-20 minutes at room temperature, stirring is performed for 20-40 minutes at 40-60° C., and then the solid is washed with an ethanol solution and dried to obtain modified nano-alumina. The modified nano-alumina is dispersed in toluene at a concentration of 0.07-0.1 g / mL and ultrasonically dispersed for 15-30 minutes; acetic acid and triethanolamine are mixed and stirred for 25-40 minutes, and then tetrabutyl titanate is added to the reactor and stirred for 2 hours. 0 to 30 minutes to obtain a mixed solution, and then slowly drop a toluene dispersion of nano-alumina into the mixed solution, continue stirring for 1.5 to 2.5 hours to obtain a sol, place the sol at room temperature for aging for 10 to 12 hours, and then dry it in an oven at 80 to 90°C, then add ethanol, ball mill for 3 to 4 hours at a rotation speed of 300 to 500 r / min, and then dry it at 80 to 90°C to obtain a modified nano-alumina / titanium oxide dual-phase filler; wherein the volume ratio of acetic acid, triethanolamine, tetrabutyl titanate, and nano-alumina dispersion is 35.5 to 38.0 mL: 2.5 to 3.2 mL: 6.8 to 7.5 mL: 20 to 25 mL.

[0018] Further, the auxiliary agent is one of diatomaceous earth or bentonite;

[0019] Furthermore, the dispersant is polyvinyl alcohol.

[0020] Furthermore, the antioxidant is at least two or more of N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine (anti-aging agent 4020), 2-mercaptobenzimidazole (anti-aging agent MB), 4,4'-bis(dimethylbenzyl)diphenylamine (anti-aging agent 445), 4,4'-dioctyldiphenylamine (anti-aging agent ODA), 2,2,4-trimethyl 1,2-dihydroquinoline polymer (anti-aging agent RD), N-phenyl-N'-isopropyl-p-phenylenediamine (anti-aging agent 4010NA) and the like.

[0021] Furthermore, the colorant is carbon black or graphite powder.

[0022] The second object of the present invention is to provide a preparation process of a self-sealing adhesive for a safety tire, wherein the materials are mixed in groups, the rubber components are added in sequence, and a continuous heating mode is adopted to improve the compatibility and dispersibility between the components. The preparation process comprises the following steps:

[0023] S1, blending the above-mentioned base material, tackifier and antioxidant, setting the temperature to 80-120° C., and stirring to obtain a mixture;

[0024] S2, add the above-mentioned inorganic filler, heat stabilizer, additive, and dispersant, continue to heat to 120-150°C and stir for a period of time;

[0025] S3, add the colorant, raise the temperature to 180-220°C, stir evenly, and evacuate to eliminate bubbles.

[0026] Furthermore, the stirring time in step S1 is 25 to 40 minutes.

[0027] Furthermore, the stirring time in step S2 is 1.5 to 3 hours.

[0028] The third object of the present invention is to provide an application of the above-mentioned sealant in the preparation of a self-sealing safety tire, wherein the application is to melt the self-sealing sealant and then spray the sealant evenly on the inner surface of the tire using a spraying device.

[0029] Furthermore, the melting temperature is 190-210° C., and the spraying thickness is 3-6 mm.

[0030] The fourth object of the present application is to provide an integrated vulcanized self-sealing safety tire, including the above-mentioned sealant layer. The tire is formed by melting the above-mentioned sealant and placing it in a roller extruder for calendering. One side is laminated and pressed with the transition layer rubber to form a rubber strip, and the other side is protected by a high-temperature resistant isolation film. The transition layer is then attached to the inner side of the innermost airtight layer of the tire. The rubber strip is positioned on the tire blank, rotated, laminated and compacted, and then formed by a tire molding machine and vulcanized together with the tire blank.

[0031] In a specific embodiment of the present application, the transition layer rubber material is composed of butyl rubber and natural rubber, EVA, C5 resin, dioctyl sebacate (DOS), calcium carbonate, kaolin, carbon black and antioxidant 2246. After mixing in a reaction kettle, heating and stirring, the material is discharged and coated, and both sides are pasted with isolation films for standby use. One side of the transition layer is attached to the sealant, and the other side is attached to the inner side of the innermost airtight layer of the tire. During the vulcanization process, the transition layer and the self-sealing glue interact with each other, the vulcanized cross-linked part of the transition layer can be cross-linked with the tire mother airtight layer, and the uncross-linked part is fused with the self-sealing glue to form a tight combination, and seamlessly fits with the tire.

[0032] The self-sealing rubber tire prepared by the present invention does not debond, flow or crack under high or low temperature conditions, thereby ensuring the balance and safety of the tire. It can prevent air leakage after nailing, and can play a role of leak-proof self-sealing. After the foreign matter is pulled out, the rubber material quickly blocks the puncture under the action of the tire pressure to slow down the air pressure loss.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The present invention provides a self-sealing rubber compound formula for a safety tire by screening rubber compound components. Under the effect of scientific matching of the components, the thermal stability of the sealant can be enhanced, so that the sealant has excellent high and low temperature resistance and can resist debonding, flow and cracking at -45°C to 120°C. The rubber compound has high deformation recovery, mechanical and self-sealing properties.

[0035] (2) The present invention adopts a composite dual-phase structure of modified alumina / titanium oxide, and uses polyvinyl pyrrolidone and sodium alginate as surface treatment agents to modify alumina, thereby improving the interaction effect between the base material and the inorganic phase. In addition, the dual-phase system promotes the dispersion of the filler in the matrix, significantly improving the mechanical properties of the sealant, and also having a positive effect on the self-sealing properties of the material.

[0036] (3) The self-sealing adhesive of the present invention can be applied in multiple ways. On the one hand, it can be sprayed on the inner wall of the tire and has high adhesion with the tire airtight layer. There is no need to perform any damaging processing on the inner wall of the tire. The inner wall of the tire only needs to be cleaned and dried to remove the mold release agent. On the other hand, it can be composited with the transition layer and then vulcanized as a whole with the tire embryo, so that the self-sealing material is formed in the embryo without any effect on the performance of the mother tire. It can also achieve good anti-puncture and anti-stab effects against sharp objects such as screws, avoid tire leakage and tire blowout, and improve driving safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is the retention rate of the elongation at break of the self-sealing adhesive materials prepared in the embodiments of the present invention and the comparative examples after high / low temperature treatment.

[0038] Figure 2 It is the adhesion retention rate of the self-sealing adhesive materials prepared in the embodiments of the present invention and the comparative examples after high / low temperature treatment. DETAILED DESCRIPTION

[0039] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Unless otherwise specified, the test methods used in the examples of the present invention are all conventional methods; the materials and reagents used, unless otherwise specified, are all reagents and materials that can be purchased from commercial channels. The relevant reagents Polyvest EP ST-E 60 (Evonik) (hereinafter referred to as ST-E60) involved in the examples and comparative examples of the present invention were purchased from Shanghai Zhuzi Industry and Trade Co., Ltd., and the hydroxy-terminated polybutadiene was purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.

[0041] The dual-phase filler used in the embodiment of the present invention is modified nano-alumina / titanium oxide, which is prepared by the following method: 45 parts of nano-alumina and 3 parts of modifiers polyvinyl pyrrolidone and sodium alginate are added to 140 parts of an aqueous solution, the mass ratio of polyvinyl pyrrolidone to sodium alginate is 4:1, ultrasonic treatment is performed at room temperature for 20 minutes, stirring at 60°C for 30 minutes, and then washing with an ethanol solution and drying the solid to obtain modified nano-alumina, the modified nano-alumina is dispersed in toluene at a concentration of 0.08 g / mL, and ultrasonic dispersion is performed for 30 minutes; acetic acid and triethanolamine are mixed and stirred. Stir for 30 minutes, then add tetrabutyl titanate to the reactor and stir for 30 minutes to obtain a mixed solution, then slowly drop the toluene dispersion of nano alumina into the mixed solution, continue stirring for 2 hours to obtain a sol, place the sol at room temperature for 10 hours, dry it in an oven at 80°C, then add ethanol, ball mill for 4 hours at a speed of 500r / min, and then dry it at 80°C to obtain a modified nano alumina / titanium oxide dual-phase filler; wherein the volume ratio of acetic acid, triethanolamine, tetrabutyl titanate, and nano alumina dispersion is 36.0mL: 3mL: 7mL: 25mL. In order to reduce the error of sample testing, the dual-phase fillers used in each embodiment and comparative example are prepared under the same conditions.

[0042] Example 1

[0043] A self-sealing rubber material for a safety tire comprises the following components in parts by weight:

[0044] 35 parts of butyl rubber, 35 parts of EPDM rubber, 5.8 parts of ST-E60, 20 parts of modified nano-alumina / titanium oxide dual-phase composite filler, 2.4 parts of zinc stearate, 1.2 parts of epoxidized soybean oil, 3.5 parts of diatomaceous earth, 1.6 parts of polyvinyl alcohol, 0.4 parts of antioxidant RD, 0.4 parts of antioxidant 4010NA, 0.4 parts of antioxidant ODA, and 0.8 parts of carbon black.

[0045] A preparation process of a self-sealing adhesive for a safety tire:

[0046] 1) Blend butyl rubber, EPDM rubber, ST-E60 and antioxidant according to the above formula, set the temperature to 110°C, and stir and mix for 30 minutes;

[0047] 2) Add dual-phase filler, zinc stearate, epoxidized soybean oil, diatomaceous earth and polyvinyl alcohol, continue to heat to 150°C and stir for 3 hours;

[0048] 3) Add carbon black, raise the temperature to 210°C, stir for 1.5 hours, and evacuate to eliminate bubbles.

[0049] Example 2

[0050] A self-sealing rubber material for a safety tire comprises the following components in parts by weight:

[0051] 26 parts of butyl rubber, 39 parts of EPDM rubber, 4.5 parts of ST-E60, 18 parts of modified nano-alumina / titanium oxide dual-phase composite filler, 2.0 parts of zinc stearate, 0.8 parts of epoxidized soybean oil, 4.5 parts of diatomaceous earth, 2.0 parts of polyvinyl alcohol, 0.4 parts of antioxidant 4020, 0.4 parts of antioxidant MB, and 1.2 parts of carbon black.

[0052] A preparation process of a self-sealing adhesive for a safety tire:

[0053] 1) Blend butyl rubber, EPDM rubber, ST-E60 and antioxidant according to the above formula, set the temperature to 120°C, and stir and mix for 25 minutes;

[0054] 2) Add dual-phase filler, zinc stearate, epoxidized soybean oil, diatomaceous earth, and polyvinyl alcohol, and continue to heat to 130°C and stir for 2h;

[0055] 3) Add carbon black, raise the temperature to 200°C, stir for 2 hours, and evacuate to eliminate bubbles.

[0056] Example 3

[0057] A self-sealing rubber material for a safety tire comprises the following components in parts by weight:

[0058] 45 parts of butyl rubber, 30 parts of EPDM rubber, 6.5 parts of ST-E60, 25 parts of modified nano-alumina / titanium oxide dual-phase composite filler, 3.0 parts of zinc stearate, 1.0 parts of epoxidized soybean oil, 4.0 parts of diatomaceous earth, 1.4 parts of polyvinyl alcohol, 0.5 parts of antioxidant 445, 0.5 parts of antioxidant MB, and 0.5 parts of carbon black.

[0059] A preparation process of a self-sealing adhesive for a safety tire:

[0060] 1) Blend butyl rubber, EPDM rubber, ST-E60 and antioxidant according to the above formula, set the temperature to 80°C, and stir and mix for 40 minutes;

[0061] 2) Add dual-phase filler, zinc stearate, epoxidized soybean oil, diatomaceous earth, and polyvinyl alcohol, and continue to heat to 120°C and stir for 3 hours;

[0062] 3) Add carbon black, raise the temperature to 180°C, stir for 3 hours, and evacuate to eliminate bubbles.

[0063] Example 4

[0064] A self-sealing rubber material for a safety tire comprises the following components in parts by weight:

[0065] 30 parts of butyl rubber, 30 parts of EPDM rubber, 4.0 parts of ST-E60, 16 parts of modified nano-alumina / titanium oxide dual-phase composite filler, 1.0 parts of zinc stearate, 1.5 parts of epoxidized soybean oil, 3.5 parts of romagnetic acid, 1.0 parts of polyvinyl alcohol, 0.5 parts of antioxidant RD, 0.5 parts of antioxidant 4010NA, 0.5 parts of antioxidant ODA, and 0.3 parts of carbon black.

[0066] A preparation process of a self-sealing adhesive for a safety tire:

[0067] 1) Blend butyl rubber, EPDM rubber, ST-E60 and antioxidant according to the above formula, set the temperature to 110°C, and stir and mix for 30 minutes;

[0068] 2) Add dual-phase filler, zinc stearate, epoxidized soybean oil, diatomaceous earth, and polyvinyl alcohol, continue to heat to 150°C and stir for 2h;

[0069] 3) Add carbon black, raise the temperature to 200°C, stir for 2 hours, and evacuate to eliminate bubbles.

[0070] Example 5

[0071] A self-sealing rubber material for a safety tire comprises the following components in parts by weight:

[0072] 29 parts of butyl rubber, 29 parts of EPDM rubber, 5.5 parts of ST-E60, 23 parts of modified nano-alumina / titanium oxide dual-phase composite filler, 2.0 parts of zinc stearate, 1.0 parts of epoxidized soybean oil, 3.0 parts of diatomaceous earth, 0.8 parts of polyvinyl alcohol, 0.2 parts of antioxidant RD, 0.2 parts of antioxidant 4010NA, and 0.8 parts of carbon black.

[0073] A preparation process and use method of a self-sealing adhesive for a safety tire:

[0074] 1) Blend butyl rubber, EPDM rubber, ST-E60 and antioxidant according to the above formula, set the temperature to 110°C, and stir and mix for 30 minutes;

[0075] 2) Add dual-phase filler, zinc stearate, epoxidized soybean oil, diatomaceous earth and polyvinyl alcohol, continue to heat to 150°C and stir for 3 hours;

[0076] 3) Add carbon black, raise the temperature to 220°C, stir for 1.5 hours, and evacuate to eliminate bubbles.

[0077] Comparative Example 1

[0078] The difference from Example 1 is that the tackifier in the rubber component is hydroxy-terminated polybutadiene instead of ST-E60 (in the same amount), and the other components, amounts and preparation process of the self-sealing adhesive are the same as those in Example 1 and will not be repeated here.

[0079] Comparative Example 2

[0080] The difference from Example 1 is that the heat stabilizer in the rubber component is a composite of calcium stearate and zinc stearate instead of zinc stearate and epoxidized soybean oil (the amount of calcium stearate is the same as that of epoxidized soybean oil), and the other components, amounts and preparation process of the self-sealing adhesive are the same as those in Example 1 and will not be repeated here.

[0081] Comparative Example 3

[0082] The difference from Example 1 is that the dual-phase filler in the rubber component is directly added with unmodified nano-alumina and titanium dioxide particles (mixed with 20 parts of the unmodified nano-alumina (40 parts) and titanium oxide (7 ml of tetrabutyl titanate hydrolyzed separately under the same conditions) in the modified nano-alumina / titanium oxide dual-phase composite in Example 1, and then replaced with an equal amount), and the other components, amounts and preparation process of the self-sealing adhesive are the same as those in Example 1 and will not be repeated here.

[0083] Comparative Example 4

[0084] The difference from Example 1 is that the dual-phase filler in the rubber component is the directly added modified nano-alumina (surface treated only with polyvinyl pyrrolidone and sodium alginate) and titanium dioxide particles (mixed according to the amount of modified nano-alumina and titanium oxide (7 ml of tetrabutyl titanate hydrolyzed separately under the same conditions) in Example 1 and then replaced with 20 equal parts), and the other components, amounts and preparation process of the self-sealing adhesive are the same as those in Example 1 and will not be repeated here.

[0085] Comparative Example 5

[0086] The difference from Example 1 is that the adhesive component lacks the auxiliary agent diatomaceous earth, and the other components, amounts and preparation process of the self-sealing adhesive are the same as those in Example 1, which will not be repeated here.

[0087] Comparative Example 6

[0088] The difference from Example 1 is that the components of the rubber material are exactly the same, but the process for preparing the self-sealing adhesive adopts a one-step mixing process, in which all the components in the formula are blended, the temperature is raised to 210° C., stirred for 5 hours, and vacuumed to eliminate bubbles.

[0089] The self-sealing adhesive materials obtained in each embodiment and comparative example were tested, and the tests included the following contents:

[0090] Detection Methods

[0091] 1. Elongation at break: The elongation at break refers to GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber". The testing machine is operated at a moving speed of 500 mm / min (tensile rate), the laboratory temperature is 27°C, and the relative humidity is 65%.

[0092] 2. Rebound rate: refer to GB1681-2009 "Determination of rebound elasticity of vulcanized rubber".

[0093] 3. Adhesion performance: The prepared self-sealing adhesive sample was melted at 210°C, and the self-sealing adhesive was evenly sprayed on the inner surface of the tire with a spraying device to a thickness of 4 mm. After cooling, it was peeled off with a DCS-500 universal testing machine to test its adhesion.

[0094] 4. Low / high temperature resistance: After the prepared rubber and tire are placed at -45℃ or 120℃ for 48 hours, their elongation at break and adhesion are tested according to methods 1 and 3, and the retention rate is used to evaluate the high and low temperature resistance; the rubber is extruded into a 5mm thick, 35mm wide and 200mm long strip, which is placed in a -45℃ low temperature treatment for 12 hours, and the strip is folded 200 times from 180° to 35° using a folding mechanism, and whether there are cracks at the bending of the strip.

[0095] 5. Self-sealing performance: Refer to GB / T38510-2020, use a tire puncture tool to puncture the tire, and test whether the punctured tire is leaking. (1) The method for observing the leak is as follows: spray foam water on the wound. If there is a leak, foam will be generated. The more serious the leak, the more foam will be generated. (2) Tire pressure measurement: puncture the tire with a screw with a diameter of 8mm and then pull it out. After an interval of 24 hours, repeat the puncture at the same position for 3 times and measure the pressure. (3) After the self-sealing tire coated with 4mm thickness is inflated to the standard air pressure and treated at -45℃ or 120℃ for 24 hours, it is immediately punctured with a screw. The foam water test is performed before and after the nail is pulled out to observe whether there are bubbles around the nail and at the extraction point.

[0096] Test results analysis

[0097] The test results of the elongation at break, rebound rate and adhesion of the self-sealing adhesive are shown in Table 1.

[0098] Table 1

[0099]

[0100]

[0101] From Table 1 and Figure 1-2 It can be seen that the rubber prepared in the embodiment of the present invention has excellent mechanical properties and thermal stability. The elongation at break and the adhesion retention rate after high and low temperature treatment can reach more than 95%, and the decline is small, indicating that the self-sealing adhesive prepared in the present application can withstand high and low temperature environments during actual use, avoiding performance degradation caused by excessively high tire temperature, and no brittle cracking occurs after low temperature treatment.

[0102] After replacing ST-E 60 with terminal hydroxyl polybutadiene in comparative example 1, the performance of the rubber compound decreased. This may be because the triethoxysilane-terminated polybutadiene has lower surface energy and high permeability, which effectively improves the wetting and dispersibility of fillers and inorganic materials in the polymer, thereby enhancing the adhesion of the rubber compound to the substrate. At the same time, it forms a network structure connected by long polyolefin chains with Si-O-Si bonds as crosslinking points. This system not only has excellent weather resistance, aging resistance and durability, but can also effectively inhibit and avoid the generation of surface cracks on the sealant after long-term use.

[0103] Compared with comparative example 2 which uses zinc stearate and calcium stearate together as heat stabilizers, the combination of zinc stearate and epoxy soybean oil can improve the thermal stability of the rubber. Zinc stearate can promote the ring-opening and cross-linking of epoxy soybean oil, and has a better synergistic effect on the mechanical properties and high and low temperature tolerance of the rubber.

[0104] The fillers used in Comparative Examples 3 and 4, dispersed modified or unmodified nano-alumina plus titanium dioxide particles, have a reduced network structure and no strong filler-rubber bond is formed, and the mechanical properties of the rubber are significantly reduced; at the same time, it is easy to cause poor compatibility and dispersibility between the filler and the base material, which increases the brittleness of the sealant, affects its low-temperature performance, and reduces its crack resistance.

[0105] Compared with Example 1, Comparative Example 5 lacks the auxiliary diatomaceous earth component. The auxiliary diatomaceous earth used in the example can reduce the moisture in the sealant, making the heat stabilizer more stable and / or the free active groups captured by the heat stabilizer more stable, further enhancing the thermal stability of the sealant, so that the sealant has excellent high and low temperature resistance.

[0106] Compared with Example 1, Comparative Example 6 adopts the traditional one-step mixing method when preparing the rubber compound, which reduces the dispersibility and compatibility between the components, making the performance of the rubber compound generally lower than that of Example 1.

[0107] Application Examples

[0108] The self-sealing adhesive prepared in this application can be used to prepare safe self-sealing tires in the following two ways:

[0109] 1. Remove the release agent from the inside of the tire, clean it and dry it, then heat the prepared self-sealing glue to 210℃ for melting, and use a spraying device to evenly spray the self-sealing glue on the inner surface of the tire with a thickness of 4mm.

[0110] 2. After the sealant is melted at 210°C, it is placed in a roller extruder for calendering to form a 4mm thick sheet, one side of which is protected by a high temperature resistant isolation film, and the other side is laminated and pressed with a transition layer rubber to form a 4.5mm thick rubber strip, and then the other side of the transition layer is attached to the inner side of the innermost airtight layer of the tire, and the rubber strip is positioned on the tire embryo, and a 42KPa pressure is used for rotation and compaction. After trimming, the isolation agent is evenly applied to the surface of the rubber strip on the bladder and the tire embryo, and the low-pressure shaping method is used for shaping. It is vulcanized at a temperature of 160°C for 45 minutes, and then placed for cooling after vulcanization. The inner high temperature isolation film is torn off to obtain an integrated vulcanized safety self-sealing tire;

[0111] The transition layer rubber is composed of 5 parts of butyl rubber, 10 parts of natural rubber, 15 parts of EVA, 15 parts of C5 resin, 12 parts of dioctyl sebacate (DOS), 5 parts of calcium carbonate, 2 parts of kaolin, 2 parts of carbon black and 1.5 parts of antioxidant 2246. After mixing at 220°C and heating and stirring in a reactor for 6 hours, the material is discharged and coated into a rubber strip with a thickness of 0.5-1mm, and both sides are pasted with isolation films for standby use.

[0112] The sealants obtained in Examples 1-3 and the comparative example of the present application were sprayed on the inner surface of the tire using Method 1; the sealants prepared in Examples 4-5 were vulcanized in the embryo positioning system using Method 2, and the performance test results are shown in Table 2.

[0113] Table 2

[0114]

[0115]

[0116] Note: The order of the amount of foam indicating the self-sealing property from strong to weak is no foam > trace > small amount > more > large amount.

[0117] As can be seen from Table 2, after the damaged tires were sprayed with foam water, no foam appeared in the tires made of the rubber of the embodiment of the present invention, indicating that the tires were airtight and had good self-sealing performance. And as can be seen from the pressure detection results in Table 2, the air pressure of the tires prepared by the present invention had almost no obvious change after being punctured and pulled out, and when the nails punctured the tires were pulled out, no rubber was seen to flow out, indicating that the rubber could recover quickly and achieve self-sealing. There was basically no air leakage after repeated punctures, and the sealing stability was good. The foam test after high and low temperature treatment also proved that the self-sealing tires prepared by the present application had good temperature tolerance, meeting the demand for tire anti-puncture self-sealing due to large temperature differences in different seasons or regions.

[0118] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the technical solution of the present invention, and are not intended to limit the specific implementation methods of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the claims of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A self-sealing rubber composition for a safety tire, characterized in that: The invention comprises the following components: base material, tackifier, inorganic filler, heat stabilizer, auxiliary agent, dispersant, antioxidant and colorant; the base material is a mixed rubber of butyl rubber and EPDM rubber, the inorganic filler is a modified nano-alumina / titanium oxide two-phase composite, and the heat stabilizer is a mixture of zinc stearate and epoxidized soybean oil.

2. The composition according to claim 1, characterized in that The components are calculated by weight as follows: 58-75 parts of base material, 4.0-6.5 parts of tackifier, 16-25 parts of inorganic filler, 2.3-4.0 parts of heat stabilizer, 3.0-4.5 parts of auxiliary agent, 0.8-2.0 parts of dispersant, 0.2-1.5 parts of antioxidant and 0.3-1.2 parts of colorant.

3. The composition according to claim 1, characterized in that The weight ratio of butyl rubber to EPDM rubber in the base material is 2:3 to 3:

2.

4. The composition according to claim 1, characterized in that The tackifier is silane-terminated modified polybutadiene rubber; the silane-terminated modified polybutadiene rubber includes triethoxysilane-terminated modified polybutadiene, and the triethoxysilane-terminated modified polybutadiene is selected from one of Polyvest EP ST-E 60 and Polyvest EP ST-E 100.

5. The composition according to claim 1, characterized in that The weight ratio of zinc stearate to epoxy soybean oil in the heat stabilizer is 2-5:1-3.

6. The composition according to claim 1, characterized in that The modified nano-alumina / titanium oxide dual-phase filler composite is prepared by the following method: using polyvinyl pyrrolidone and sodium alginate as surface treatment agents to modify nano-alumina, and then dispersing the nano-alumina in toluene; mixing acetic acid and triethanolamine, adding tetrabutyl titanate and stirring to obtain a mixed solution, then adding a toluene dispersion of nano-alumina to the mixed solution, continuing to stir to obtain a sol, aging and drying the sol, and then grinding to obtain the composite.

7. The composition according to claim 1, characterized in that The auxiliary agent is diatomaceous earth or bentonite; the dispersant is polyvinyl alcohol; the antioxidant is two or more of N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine, 2-mercaptobenzimidazole, 4,4'-bis(dimethylbenzyl)diphenylamine, 4,4'-dioctyldiphenylamine, 2,2,4-trimethyl-1,2-dihydroquinoline polymer, and N-phenyl-N'-isopropyl-p-phenylenediamine antioxidant; and the colorant is carbon black or graphite powder.

8. A process for preparing a self-sealing adhesive for a safety tire, characterized in that: The self-sealing adhesive is prepared from the adhesive composition according to any one of claims 1 to 7, and the preparation process comprises the following steps: S1. Blend the base material, tackifier and antioxidant, set the temperature to 80-120° C., and stir evenly to obtain a mixture; S2. Add inorganic filler, heat stabilizer, additive and dispersant to the mixture, continue to heat to 120-150°C and stir for a while; S3, adding colorant, raising the temperature to 180-220°C, stirring evenly, and vacuuming to eliminate bubbles to obtain the self-sealing adhesive.

9. Use of a self-sealing adhesive in preparing a self-sealing safety tire, characterized in that: The self-sealing adhesive is obtained by the preparation process described in claim 8, and the application is to melt the self-sealing adhesive and then spray the adhesive evenly on the inner surface of the tire using a spraying device.

10. An integrated vulcanized self-sealing safety tire, characterized in that: The method comprises the following steps: the self-sealing adhesive is obtained by the preparation process of claim 8, the self-sealing adhesive is melted and then placed in a roller extruder for calendering, and then laminated and pressed with a transition layer adhesive to form a rubber strip, and then the transition layer is laminated to the inner side of the innermost airtight layer of the tire, the rubber strip is positioned on the tire blank, rotated, laminated and compacted, and then formed by a tire molding machine and vulcanized together with the tire blank to obtain the obtained product.

Citation Information

Patent Citations

  • Self-sealing safety tire mixed polymer memory glue and preparation method thereof

    CN116693951A

  • Self-sealing rubber composition and preparation method thereof

    CN118325245A

  • Aluminum fin material for heat exchanger

    JP2002241963A

  • Resin aqueous dispersion, resin particle, colored resin particle and toner

    JP2016190916A

  • Resin particle, composite resin particle and method for producing toner

    JP2018087320A