Epoxy resin adhesive with ultralow expansion coefficient and preparation method thereof
By using a combination of ultra-low expansion coefficient epoxy resin and modified ceramic filler in adhesives, the problems of insufficient temperature change sensitivity and large internal stress in existing adhesives in extreme environments are solved, and higher strength and heat resistance are achieved Performance, suitable for aerospace and chip semiconductor fields.
Patent Information
- Application Number
- CN202411081705.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
AI Technical Summary
In the fields of aerospace and chip semiconductors, existing adhesives are difficult to meet the requirements of temperature change sensitivity in extreme environments, and the internal stress increases due to the difference in expansion coefficient between the substrate and the adhesive, which affects strength and heat shock resistance.
Using ultra-low expansion coefficient epoxy resin adhesive, a combination of low expansion coefficient ceramic filler and epoxy resin modified by silane coupling agent is used, combined with appropriate diluent and curing agent, the expansion coefficient and viscosity are adjusted to reduce the thermal expansion of the adhesive coefficients and cure through specific proportions and process steps.
It improves the sensitivity of the measurement components to temperature changes, reduces internal stress, enhances the strength and heat shock resistance of the adhesive, and meets the high precision and high quality requirements in the fields of aerospace and chip semiconductors.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, in particular to an ultra-low expansion coefficient epoxy resin adhesive and a preparation method thereof. Background Art
[0002] Adhesives are mainly used in the aerospace field and the chip semiconductor field. With the advancement of science and technology, the selection of aerospace materials has become more stringent. Aerospace products operate in extreme environments and require adhesives to withstand ultra-low temperatures, high vacuums, thermal cycles and ultraviolet rays. Measuring elements using ordinary adhesives are insensitive to temperature changes within a certain high temperature range, and the displacement changes are not obvious, making it difficult to meet the measurement accuracy requirements. In the chip semiconductor field, due to the large difference in the linear expansion coefficient between the substrate and the epoxy adhesive, the molding curing shrinkage and thermal shrinkage during the curing process will cause internal stress in the application material, resulting in various defects such as decreased strength, poor thermal shock resistance, aging cracking, voids, passivation and delamination.
[0003] Therefore, it is necessary to provide an improved adhesive suitable for the aerospace field and the chip semiconductor field. Summary of the invention
[0004] The object of the present invention is to provide an ultra-low expansion coefficient epoxy resin adhesive and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: an ultra-low expansion coefficient epoxy resin adhesive, comprising component A, component B and component C; Component A is a low expansion coefficient ceramic filler modified by a silane coupling agent, component B includes a mixed resin of an epoxy resin and a reactive diluent, and component C is a curing agent; The silane coupling agent includes any one or a combination of KH550, KH560 and KH570; The low expansion coefficient ceramic filler includes spodumene (LiAl(SiO3)2 / Li2O·Al2O3·4SiO2), eucryptite (β-LiAISiO4), cordierite (Mg2Al4Si5O 18 ), zirconium tungstate (ZrW2O8), aluminum titanate (Al2TiO5), zirconium phosphate (Zr2P2O9), magnesium phosphate (Mg2P4O7), NaZr2(PO4)3 (abbreviated as NZP), BaZr4(PO4)6, any one or a combination of several thereof.
[0006] The grain size of the low expansion coefficient ceramic filler is 1 μm-20 μm.
[0007] The epoxy resin in component B includes linear aliphatic epoxy resin, glycidyl ether epoxy resin, glycidyl ester epoxy resin, and glycidyl amine epoxy resin.
[0008] The functionality of the glycidyl ether epoxy resin is difunctional or trifunctional, the epoxy value of the epoxy resin is 0.5 to 0.9, and the viscosity of the epoxy resin is 300 to 700 mPa.s.
[0009] The active diluent in component B includes any one or more combinations of ethylene glycol diglycidyl ether, butanediol diglycidyl ether, polyethanol diglycidyl ether, polypropylene glycol diglycidyl ether or n-butyl glycidyl ether.
[0010] The curing agent includes any one or more combinations of aliphatic amine curing agents, alicyclic amine curing agents, aromatic amine curing agents or imidazole curing agents, the aliphatic amine curing agent includes any one or more combinations of diethylenetriamine, ethylenediamine or hexamethylenediamine, the alicyclic amine curing agent includes menthane diamine and / or isophorone diamine, the aromatic amine curing agent includes any one or more combinations of m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone or diethyltoluenediamine, and the imidazole curing agent includes any one or more combinations of 2-methylimidazole, 1-aminoethyl-2-methylimidazole or 2-methyl-4-ethylimidazole.
[0011] The present invention also provides a method for preparing an ultra-low expansion coefficient epoxy resin adhesive, comprising the following steps: S1: mixing the silane coupling agent with the solvent, adding the low expansion coefficient ceramic filler after dissolving, heating to react, and filtering to obtain component A after cooling; S2: mixing the epoxy resin and the reactive diluent to obtain component B; S3: Mix component A, component B and component C thoroughly according to the ratio, apply to the surface to be bonded, and cure after heating.
[0012] The solvent in S1 is deionized water or ethanol, the mixing step is carried out under stirring, the mixing time is 10-30 minutes, the heating temperature is 60-80°C, the heating time is 20-60 minutes, and the mass ratio of the low expansion coefficient ceramic filler, the silane coupling agent and the solvent in S1 is 100:(0.5-5):(500-800).
[0013] The mass ratio of the epoxy resin to the reactive diluent in S2 is (8:2) to (5:5).
[0014] The weight proportions of component A, component B, component C and solvent in S3 are 500-1000 parts, 100 parts, 3-20 parts and 0-200 parts respectively; the solvent in S3 includes any one of acetone, ethanol, N,N-dimethylformamide or N-methylpyrrolidone, the mixing method is high-speed stirring or three-roll grinding, the curing heating temperature is 60-100°C, and the curing time is 1-6h.
[0015] Compared with the prior art, the present invention has the following beneficial effects: In the aerospace field, by using ultra-low thermal expansion coefficient bonding materials, the sensitivity of measuring elements to temperature changes is improved, and displacement changes are manifested to meet the requirements of measurement accuracy.
[0016] In the chip semiconductor field, by reducing the linear expansion coefficient of the adhesive and minimizing the difference in linear expansion coefficient between the adhesive and the application material, internal stress can be reduced, strength can be increased, thermal shock resistance can be enhanced, and the overall quality of the product can be improved. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] The present invention provides a technical solution: an ultra-low expansion coefficient epoxy resin adhesive, comprising component A, component B and component C; Component A is a low expansion coefficient ceramic filler modified with a silane coupling agent, which can significantly reduce the thermal expansion coefficient of the adhesive. By adjusting the average particle size of the low expansion coefficient ceramic filler, an adhesive product with both low expansion characteristics and bonding strength can be obtained; if the particle size is too small, the filling amount will be reduced, affecting the thermal expansion performance; if the particle size is too large, it will affect the bonding strength.
[0019] Component B includes a mixed resin of epoxy resin and a reactive diluent. By adding the reactive diluent, the viscosity of the resin component is reduced, thereby increasing the filling amount of the low expansion ceramic filler.
[0020] The silane coupling agent includes any one or a combination of KH550, KH560 and KH570; The low expansion coefficient ceramic filler includes spodumene (LiAl(SiO3)2 / Li2O·Al2O3·4SiO2), eucryptite (β-LiAISiO4), cordierite (Mg2Al4Si5O 18), zirconium tungstate (ZrW2O8), aluminum titanate (Al2TiO5), zirconium phosphate (Zr2P2O9), magnesium phosphate (Mg2P4O7), NaZr2(PO4)3 (abbreviated as NZP), BaZr4(PO4)6, any one or a combination of several thereof.
[0021] The grain size of the low expansion coefficient ceramic filler is 1 μm-20 μm.
[0022] The epoxy resin in component B includes linear aliphatic epoxy resin, glycidyl ether epoxy resin, glycidyl ester epoxy resin, and glycidyl amine epoxy resin.
[0023] The functionality of the glycidyl ether epoxy resin is difunctional or trifunctional, the epoxy value of the epoxy resin is 0.5-0.9, and the viscosity of the epoxy resin is 300-700 mPa.s. The epoxy value and viscosity of the epoxy resin are adjusted to meet the process requirements of actual application scenarios. Too high viscosity will reduce the filling amount of low expansion coefficient ceramic filler and affect thermal expansion performance. Too low viscosity will reduce the bonding processability.
[0024] The active diluent in component B includes any one or more combinations of ethylene glycol diglycidyl ether, butanediol diglycidyl ether, polyethanol diglycidyl ether, polypropylene glycol diglycidyl ether or n-butyl glycidyl ether. The active diluent has the advantages of low viscosity and high compatibility with the main resin.
[0025] Component C is a curing agent, including any one or more combinations of aliphatic amine curing agents, alicyclic amine curing agents, aromatic amine curing agents or imidazole curing agents.
[0026] The fatty amine curing agent includes any one or more combinations of diethylenetriamine, ethylenediamine or hexamethylenediamine, the alicyclic amine curing agent includes menthane diamine and / or isophorone diamine, the aromatic amine curing agent includes any one or more combinations of m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone or diethyltoluenediamine, and the imidazole curing agent includes any one or more combinations of 2-methylimidazole, 1-aminoethyl-2-methylimidazole or 2-methyl-4-ethylimidazole.
[0027] The present invention also provides a method for preparing an ultra-low expansion coefficient epoxy resin adhesive, comprising the following steps: S1: mixing the silane coupling agent with the solvent, adding the low expansion coefficient ceramic filler after dissolving, heating to react, and filtering to obtain component A after cooling; S2: mixing the epoxy resin and the reactive diluent to obtain component B; S3: Mix component A, component B and component C thoroughly according to the ratio, apply to the surface to be bonded, and cure after heating.
[0028] The solvent in S1 is deionized water or ethanol, the mixing step is carried out under stirring, the mixing time is 10-30 minutes, the heating temperature is 60-80°C, the heating time is 20-60 minutes, and the mass ratio of the low expansion coefficient ceramic filler, the silane coupling agent and the solvent in S1 is 100:(0.5-5):(500-800).
[0029] By adjusting the mass ratio of the low expansion coefficient ceramic filler, the silane coupling agent and the solvent described in S1, the silane coupling agent can evenly coat the low expansion coefficient ceramic filler. If the mass ratio of the silane coupling agent is too low, the low expansion coefficient ceramic filler will not be completely modified. If the mass ratio is too high, the excess silane coupling agent cannot be removed, affecting the comprehensive performance of the low expansion adhesive. If the mass ratio of the solvent is too low, the low expansion coefficient ceramic filler cannot be evenly dispersed, affecting the uniformity of the product. If the mass ratio is too high, the reaction time will be greatly increased. The mass ratio of the epoxy resin to the active diluent in S2 is (8:2) to (5:5). By adjusting the mass ratio of the epoxy resin to the active diluent in S2, component B with a balanced epoxy value and viscosity is obtained. If the mass ratio is too low, the epoxy value will be reduced, affecting the bonding strength of the low expansion adhesive. Otherwise, the viscosity of the system will be too high, the filling amount of the low expansion coefficient ceramic filler will be reduced, and the thermal expansion properties of the adhesive will be affected.
[0030] The weight proportions of component A, component B, component C and solvent in S3 are 500-1000 parts, 100 parts, 3-20 parts and 0-200 parts respectively. The weight proportion of component A is adjusted to achieve an optimal ratio between the low expansion coefficient ceramic filler and component B. If the weight proportion of component A is too low, it will affect the thermal expansion performance, otherwise it will affect the bonding strength. The weight proportion of the curing agent is adjusted to achieve an optimal ratio between the curing agent and component B. If the weight proportion of the curing agent is too low, a higher curing temperature and curing time will be required, and the low expansion adhesive may not be completely cured. Otherwise, the curing reaction will be too violent, affecting the mechanical properties, and even an implosion reaction will occur.
[0031] The solvent in S3 includes any one of acetone, ethanol, N,N-dimethylformamide or N-methylpyrrolidone, the mixing method is high-speed stirring or three-roll grinding, the curing heating temperature is 60-100° C., and the curing time is 1-6 hours. Example 1
[0032] This embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of which include component A and component B; component A is cordierite (Mg2Al4Si5O 18) ceramic filler; the component B comprises a combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 and a mixed resin of ethylene glycol diglycidyl ether.
[0033] The preparation method of the ultra-low expansion adhesive is as follows: Stir KH550 silane coupling agent with deionized water for 20 min, and add cordierite (Mg2Al4Si5O 18 ) ceramic filler, heated at 70°C for 40 min to react, cooled and filtered with deionized water to obtain component A, in which cordierite (Mg2Al4Si5O 18 ) The mass ratio of ceramic filler, KH550 silane coupling agent and deionized water is 100:3:600; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the ethylene glycol diglycidyl ether reactive diluent is 6:4, to obtain component B; 750 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing m-phenylenediamine (MPD) and 2-methyl-4-ethylimidazole, and 50 parts of acetone were mixed, and the mixture was heated at 80° C. for 2 hours to undergo a curing reaction to obtain the adhesive. Example 2
[0034] The present embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of the adhesive include component A and component B; component A is spodumene (LiAl(SiO3)2 / Li2O·Al2O3·4SiO2) ceramic filler modified by KH550 silane coupling agent; component B includes a combination of trifunctional glycidyl ester type epoxy resin MY0510 and difunctional glycidyl ether type epoxy resin E51 and a mixed resin of ethylene glycol diglycidyl ether.
[0035] The preparation method of the ultra-low expansion adhesive is as follows: Stirring KH550 silane coupling agent and deionized water for 20 minutes, adding spodumene (LiAl(SiO3)2 / Li2O·Al2O3·4SiO2) ceramic filler with an average particle size of 15 μm after dissolution, heating at 70°C for 50 minutes for reaction, and filtering with deionized water after cooling to obtain component A, wherein the mass ratio of spodumene (LiAl(SiO3)2 / Li2O·Al2O3·4SiO2) ceramic filler, KH550 silane coupling agent and deionized water is 100:3:700; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the ethylene glycol diglycidyl ether reactive diluent is 6:4, to obtain component B; 750 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing m-phenylenediamine (MPD) and 2-methyl-4-ethylimidazole, and 50 parts of acetone were mixed, and the mixture was heated at 80° C. for 2 hours to undergo a curing reaction to obtain the adhesive. Example 3
[0036] The present embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of the adhesive include component A and component B; component A is a eucryptite (β-LiAISiO4) ceramic filler modified by a KH550 silane coupling agent; component B includes a combination of a trifunctional glycidyl ester type epoxy resin MY0510 and a difunctional glycidyl ether type epoxy resin E51 and a mixed resin of ethylene glycol diglycidyl ether.
[0037] The preparation method of the ultra-low expansion adhesive is as follows: Stirring KH550 silane coupling agent and deionized water for 20 minutes, adding eucryptite (β-LiAISiO4) ceramic filler with an average particle size of 12 μm after dissolution, heating at 70°C for 50 minutes for reaction, and filtering with deionized water after cooling to obtain component A, wherein the mass ratio of eucryptite (β-LiAISiO4) ceramic filler, KH550 silane coupling agent and deionized water is 100:3:600; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the ethylene glycol diglycidyl ether reactive diluent is 6:4, to obtain component B; 750 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing m-phenylenediamine (MPD) and 2-methyl-4-ethylimidazole, and 50 parts of acetone were mixed, and the mixture was heated at 80° C. for 2 hours to undergo a curing reaction to obtain the adhesive. Example 4
[0038] This embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of which include component A and component B; component A is cordierite (Mg2Al4Si5O 18 ) ceramic filler; the component B comprises a combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 and a mixed resin of ethylene glycol diglycidyl ether.
[0039] The preparation method of the ultra-low expansion adhesive is as follows: Stir KH550 silane coupling agent with deionized water for 20 min, and add cordierite (Mg2Al4Si5O 18 ) ceramic filler, heated at 70°C for 40 min to react, cooled and filtered with deionized water to obtain component A, in which cordierite (Mg2Al4Si5O 18 ) The mass ratio of ceramic filler, KH550 silane coupling agent and deionized water is 100:3:600; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the ethylene glycol diglycidyl ether reactive diluent is 6:4, to obtain component B; 750 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing m-phenylenediamine (MPD) and 2-methyl-4-ethylimidazole, and 50 parts of acetone were mixed, and the mixture was heated at 80° C. for 2 hours to undergo a curing reaction to obtain the adhesive. Example 5
[0040] This embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of which include component A and component B; component A is cordierite (Mg2Al4Si5O 18 ) ceramic filler; the component B comprises a combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 and a mixed resin of ethylene glycol diglycidyl ether.
[0041] The preparation method of the ultra-low expansion adhesive is as follows: Stir KH550 silane coupling agent with deionized water for 20 min, and add cordierite (Mg2Al4Si5O 18 ) ceramic filler, heated at 70°C for 40 min to react, cooled and filtered with deionized water to obtain component A, in which cordierite (Mg2Al4Si5O 18 ) The mass ratio of ceramic filler, KH550 silane coupling agent and deionized water is 100:3:600; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the butanediol diglycidyl ether reactive diluent is 6:4, to obtain component B; 750 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing m-phenylenediamine (MPD) and 2-methyl-4-ethylimidazole, and 50 parts of acetone were mixed, and the mixture was heated at 80° C. for 2 hours to undergo a curing reaction to obtain the adhesive. Example 6
[0042] This embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of which include component A and component B; component A is cordierite (Mg2Al4Si5O 18 ) ceramic filler; the component B comprises a combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 and a mixed resin of ethylene glycol diglycidyl ether.
[0043] The preparation method of the ultra-low expansion adhesive is as follows: Stir KH550 silane coupling agent with deionized water for 20 min, and add cordierite (Mg2Al4Si5O 18) ceramic filler, heated at 70°C for 40 min to react, cooled and filtered with deionized water to obtain component A, in which cordierite (Mg2Al4Si5O 18 ) The mass ratio of ceramic filler, KH550 silane coupling agent and deionized water is 100:3:600; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the ethylene glycol diglycidyl ether reactive diluent is 6:4, to obtain component B; 750 parts of component A, 100 parts of component B, 15 parts of a curing agent (component C) prepared by mixing diethyltoluenediamine (DETDA) and 2-methyl-4-ethylimidazole, and 50 parts of acetone were mixed, and the mixture was heated at 80° C. for 2 hours to undergo a curing reaction to obtain the adhesive. Example 7
[0044] This embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of which include component A and component B; component A is cordierite (Mg2Al4Si5O 18 ) ceramic filler; the component B comprises a combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 and ethylene glycol diglycidyl ether.
[0045] The preparation method of the adhesive is as follows: Stir KH550 silane coupling agent with deionized water for 20 min, and add cordierite (Mg2Al4Si5O 18 ) ceramic filler, heated at 70°C for 40 min to react, cooled and filtered with deionized water to obtain component A, in which cordierite (Mg2Al4Si5O 18 ) The mass ratio of ceramic filler, KH550 silane coupling agent and deionized water is 100:2:600; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the ethylene glycol diglycidyl ether reactive diluent is 7:3, to obtain component B; 500 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing diethyltoluenediamine (DETDA) and 2-methyl-4-ethylimidazole, and 0 parts of acetone were mixed, and the mixture was heated at 80° C. for 4 hours to undergo a curing reaction to obtain the adhesive. Example 8
[0046] This embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of which include component A and component B; component A is cordierite (Mg2Al4Si5O 18 ) ceramic filler; the component B comprises a combination of a trifunctional glycidyl ester epoxy resin TDE85 and a difunctional glycidyl ether epoxy resin E44 and ethylene glycol diglycidyl ether.
[0047] The preparation method of the adhesive is as follows: Stir KH550 silane coupling agent with deionized water for 20 min, and add cordierite (Mg2Al4Si5O 18 ) ceramic filler, heated at 70°C for 40 min to react, cooled and filtered with deionized water to obtain component A, in which cordierite (Mg2Al4Si5O 18 ) The mass ratio of ceramic filler, KH550 silane coupling agent and deionized water is 100:5:750; A compound of a trifunctional glycidyl ester epoxy resin TDE85 having an epoxy value of 0.75 and a difunctional glycidyl ether epoxy resin E44 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the compound of the trifunctional glycidyl ester epoxy resin TDE85 and the difunctional glycidyl ether epoxy resin E44 to the ethylene glycol diglycidyl ether reactive diluent is 7:3, to obtain component B; 1000 parts of component A, 100 parts of component B, 15 parts of a curing agent (component C) prepared by mixing diethyltoluenediamine (DETDA) and 2-methyl-4-ethylimidazole, and 100 parts of acetone were mixed, and the mixture was heated at 80° C. for 6 hours to undergo a curing reaction to obtain the adhesive. Example 9
[0048] This embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of the adhesive include component A and component B; component A is a magnesium phosphate (Mg2P4O7) ceramic filler modified by a KH560 silane coupling agent; component B includes a trifunctional glycidyl ester type epoxy resin TDE85 and polyethylene glycol diglycidyl ether.
[0049] The preparation method of the adhesive is as follows: Stirring KH560 silane coupling agent and ethanol for 10 minutes, adding magnesium phosphate (Mg2P4O7) ceramic filler with an average particle size of 15 μm after dissolution, heating at 60°C for 60 minutes for reaction, and filtering with deionized water after cooling to obtain component A, wherein the mass ratio of magnesium phosphate (Mg2P4O7) ceramic filler, KH560 silane coupling agent and ethanol is 100:0.5:500; A trifunctional glycidyl ester epoxy resin TDE85 having an epoxy value of 0.85 and a polyethylene glycol diglycidyl ether active diluent are mixed, wherein the mass ratio of the trifunctional glycidyl ester epoxy resin TDE85 to the polyethylene glycol diglycidyl ether active diluent is 5:5, to obtain component B; 1500 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing diethyltoluenediamine (DETDA) and 2-methylimidazole, and 100 parts of ethanol were mixed, and the mixture was heated at 60° C. for 3 hours to undergo a curing reaction to obtain the adhesive. Example 10
[0050] This embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of the adhesive include component A and component B; component A is a magnesium phosphate (Mg2P4O7) ceramic filler modified by a KH560 silane coupling agent; component B includes a difunctional glycidyl ether type epoxy resin E51 and polyethylene glycol diglycidyl ether.
[0051] The preparation method of the adhesive is as follows: Stirring KH560 silane coupling agent and ethanol for 30 minutes, adding magnesium phosphate (Mg2P4O7) ceramic filler with an average particle size of 20 μm after dissolution, heating at 80°C for 20 minutes for reaction, and filtering with deionized water after cooling to obtain component A, wherein the mass ratio of magnesium phosphate (Mg2P4O7) ceramic filler, KH560 silane coupling agent and ethanol is 100:5:750; Mixing a trifunctional glycidyl ester epoxy resin E51 having an epoxy value of 0.55 and a polyethylene glycol diglycidyl ether active diluent, wherein the mass ratio of the trifunctional glycidyl ester epoxy resin to the polyethylene glycol diglycidyl ether active diluent is 5:5, to obtain component B; 500 parts of component A, 100 parts of component B, 3 parts of a curing agent prepared by mixing diethyltoluenediamine (DETDA) and 2-methyl-4-ethylimidazole, and 0 parts of ethanol were mixed, and the mixture was heated at 100° C. for 2 hours to undergo a curing reaction, and then the adhesive was obtained. Embodiment 11
[0052] The present embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of the adhesive include component A and component B; component A is BaZr4(PO4)6 ceramic filler modified by KH550 silane coupling agent; component B includes a combination of trifunctional glycidyl ester type epoxy resin MY0510 and difunctional glycidyl ether type epoxy resin E51 and a mixed resin of ethylene glycol diglycidyl ether.
[0053] The preparation method of the ultra-low expansion adhesive is as follows: Stirring KH550 silane coupling agent and deionized water for 20 minutes, adding BaZr4(PO4)6 ceramic filler with an average particle size of 10 μm after dissolution, heating at 70°C for 40 minutes for reaction, and filtering with deionized water after cooling to obtain component A, wherein the mass ratio of BaZr4(PO4)6 ceramic filler, KH550 silane coupling agent and deionized water is 100:3:600; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the ethylene glycol diglycidyl ether reactive diluent is 6:4, to obtain component B; 750 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing m-phenylenediamine (MPD) and 2-methyl-4-ethylimidazole, and 50 parts of acetone were mixed, and the mixture was heated at 80° C. for 2 hours to undergo a curing reaction to obtain the adhesive. Example 12
[0054] The present embodiment provides an ultra-low expansion coefficient adhesive, the raw materials of the adhesive include component A and component B; component A is NaZr2(PO4)3 ceramic filler modified by KH550 silane coupling agent; component B includes a combination of trifunctional glycidyl ester type epoxy resin MY0510 and difunctional glycidyl ether type epoxy resin E51 and a mixed resin of ethylene glycol diglycidyl ether.
[0055] The preparation method of the ultra-low expansion adhesive is as follows: Stirring KH550 silane coupling agent and deionized water for 20 minutes, adding NaZr2(PO4)3 ceramic filler with an average particle size of 10 μm after dissolution, heating at 70°C for 40 minutes for reaction, and filtering with deionized water after cooling to obtain component A, wherein the mass ratio of NaZr2(PO4)3 ceramic filler, KH550 silane coupling agent and deionized water is 100:3:600; A combination of a trifunctional glycidyl ester epoxy resin MY0510 and a difunctional glycidyl ether epoxy resin E51 having an epoxy value of 0.75 and an ethylene glycol diglycidyl ether reactive diluent are mixed, wherein the mass ratio of the combination of the trifunctional glycidyl ester epoxy resin MY0510 and the difunctional glycidyl ether epoxy resin E51 to the ethylene glycol diglycidyl ether reactive diluent is 6:4, to obtain component B; 750 parts of component A, 100 parts of component B, 10 parts of a curing agent (component C) prepared by mixing m-phenylenediamine (MPD) and 2-methyl-4-ethylimidazole, and 50 parts of acetone were mixed, and the mixture was heated at 80° C. for 2 hours to undergo a curing reaction to obtain the adhesive.
[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An ultra-low expansion coefficient epoxy resin adhesive, characterized in that: Comprising component A, component B and component C; Component A is a low expansion coefficient ceramic filler modified by a silane coupling agent, component B includes a mixed resin of an epoxy resin and a reactive diluent, and component C is a curing agent; The silane coupling agent includes any one or a combination of KH550, KH560 and KH570; The low expansion coefficient ceramic filler includes spodumene (LiAl(SiO3)2 / Li2O·Al2O3·4SiO2), eucryptite (β-LiAISiO4), cordierite (Mg2Al4Si5O 18 ), zirconium tungstate (ZrW2O8), aluminum titanate (Al2TiO5), zirconium phosphate (Zr2P2O9), magnesium phosphate (Mg2P4O7), NaZr2(PO4)3 (abbreviated as NZP), BaZr4(PO4)6, any one or a combination of several thereof.
2. The ultra-low expansion coefficient epoxy resin adhesive according to claim 1, characterized in that: The grain size of the low expansion coefficient ceramic filler is 1 μm-20 μm.
3. The ultra-low expansion coefficient epoxy resin adhesive according to claim 1, characterized in that: The epoxy resin in component B includes linear aliphatic epoxy resin, glycidyl ether epoxy resin, glycidyl ester epoxy resin, and glycidyl amine epoxy resin.
4. The ultra-low expansion coefficient epoxy resin adhesive according to claim 3, characterized in that: The functionality of the glycidyl ether epoxy resin is difunctional or trifunctional, the epoxy value of the epoxy resin is 0.5 to 0.9, and the viscosity of the epoxy resin is 300 to 700 mPa.s.
5. The ultra-low expansion coefficient epoxy resin adhesive according to claim 1, characterized in that: The active diluent in component B includes any one or more combinations of ethylene glycol diglycidyl ether, butanediol diglycidyl ether, polyethanol diglycidyl ether, polypropylene glycol diglycidyl ether or n-butyl glycidyl ether.
6. The ultra-low expansion coefficient epoxy resin adhesive according to claim 1, characterized in that: The curing agent includes any one or more combinations of aliphatic amine curing agents, alicyclic amine curing agents, aromatic amine curing agents or imidazole curing agents, the aliphatic amine curing agent includes any one or more combinations of diethylenetriamine, ethylenediamine or hexamethylenediamine, the alicyclic amine curing agent includes menthane diamine and / or isophorone diamine, the aromatic amine curing agent includes any one or more combinations of m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone or diethyltoluenediamine, and the imidazole curing agent includes any one or more combinations of 2-methylimidazole, 1-aminoethyl-2-methylimidazole or 2-methyl-4-ethylimidazole.
7. A method for preparing an ultra-low expansion coefficient epoxy resin adhesive, characterized in that: The method for preparing the ultra-low expansion coefficient epoxy resin adhesive according to any one of claims 1 to 6 comprises the following steps: S1: mixing the silane coupling agent with the solvent, adding the low expansion coefficient ceramic filler after dissolving, heating to react, and filtering to obtain component A after cooling; S2: mixing the epoxy resin and the reactive diluent to obtain component B; S3: Mix component A, component B and component C thoroughly according to the ratio, apply to the surface to be bonded, and cure after heating.
8. The method for preparing an ultra-low expansion coefficient epoxy resin adhesive according to claim 7, characterized in that: The solvent in S1 is deionized water or ethanol, the mixing step is carried out under stirring, the mixing time is 10-30 minutes, the heating temperature is 60-80°C, the heating time is 20-60 minutes, and the mass ratio of the low expansion coefficient ceramic filler, the silane coupling agent and the solvent in S1 is 100:(0.5-5):(500-800).
9. The method for preparing an ultra-low expansion coefficient epoxy resin adhesive according to claim 7, characterized in that: The mass ratio of the epoxy resin to the reactive diluent in S2 is (8:2) to (5:5).
10. The method for preparing an ultra-low expansion coefficient epoxy resin adhesive according to claim 7, characterized in that: The weight proportions of component A, component B, component C and solvent in S3 are 500-1000 parts, 100 parts, 3-20 parts and 0-200 parts respectively; the solvent in S3 includes any one of acetone, ethanol, N,N-dimethylformamide or N-methylpyrrolidone, the mixing method is high-speed stirring or three-roll grinding, the curing heating temperature is 60-100°C, and the curing time is 1-6h.
Citation Information
Cited By