Adhesive for electronic precision device and preparation method thereof

By using naphthyl epoxy resin, silicone and OH-BN/A l N/PLGA-PEG-NH2 composite materials in the adhesive, combined with a modified polythiol curing agent, the unstable curing of thermally conductive adhesive at room temperature is solved. The problem of this problem is to achieve rapid curing and high thermal conductivity of adhesives, meeting the high-efficiency bonding and heat dissipation needs of electronic precision devices.

CN118931450AInactive Publication Date: 2024-11-12GUANGDONG YAQIAO NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411195425.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing thermally conductive adhesives are unstable in curing at room temperature, their viscosity increases, and curing requires high temperatures, making it difficult to meet the high requirements of electronic precision devices for thermal conductivity and adhesion.

Method used

Using a combination of naphthyl epoxy resin, silicone, OH-BN/A l N/PLGA-PEG-NH2 composite material and modified polythiol curing agent, the mixture of modified polythiol curing agents A and B and silane coupling agent to form a composite curing agent to achieve rapid curing and high thermal conductivity of the adhesive at room temperature.

Benefits of technology

It achieves rapid curing of adhesive at room temperature, good storage stability, excellent thermal conductivity, and is suitable for efficient bonding and heat dissipation needs of electronic precision devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005016234770000101
    Figure BDA0005016234770000101
  • Figure BDA0005016234770000111
    Figure BDA0005016234770000111
  • Figure BDA0005016234770000112
    Figure BDA0005016234770000112
Patent Text Reader

Abstract

The invention discloses an adhesive for an electronic precision device. The adhesive comprises the following components in parts by weight: 80-100 parts of naphthyl epoxy resin, 5-30 parts of siloxane, 5-25 parts of a diluent, 10-50 parts of an insulating heat-conducting material and 3-20 parts of a composite curing agent, the insulating and heat conducting material is an OH-BN / AlN / PLGA-PEG-NH2 composite material, and the insulating and heat conducting material is a composite material; the composite curing agent comprises a modified polythiol curing agent A and a modified polythiol curing agent B, the modified polythiol curing agent A and the modified polythiol curing agent B are mixed according to the mass ratio of (1-2.5): (1-2.5), 0.05%-1% of a silane coupling agent is added, stirring is conducted, and the composite curing agent is obtained. The adhesive prepared by the invention has excellent adhesive property and good heat-conducting property, is high in normal-temperature curing speed, and has a relatively good application prospect in the field of electronic and electrical appliances.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and in particular to an adhesive for electronic precision devices and a preparation method thereof. Background Art

[0002] With the development of science and technology, the use of thermal conductive adhesives has become more and more extensive, such as in the aerospace field, mobile communications, new energy vehicles, medical equipment, electronic appliances and other related fields. Polymer composites combine the advantages of polymer matrix and thermal conductive fillers, and play a vital role in the use of today's electronic equipment. The development trend of electronic products is increasingly miniaturized and functionally integrated, which puts higher and higher requirements on the heat dissipation system.

[0003] At present, the thermal conductivity of thermally conductive adhesives is mainly achieved by filling thermally conductive powder. Thermally conductive powders mainly include aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon nitride, silicon carbide, carbon fiber and graphene, which form a random dispersion state in the adhesive, causing problems such as low strength of the adhesive. Epoxy resin is widely used in semiconductor and electronic packaging materials due to its excellent mechanical, electrical and heat resistance properties. Single-component epoxy adhesives are easy to use and can be directly extruded for use. However, the single-component epoxy resin adhesives circulating on the market use a latent curing agent, which has poor storage stability, is prone to viscosity increase, and the glue solidifies, and generally requires high temperature curing.

[0004] Therefore, there is still a need to develop a one-component adhesive that can be cured at room temperature and has good thermal conductivity. Summary of the invention

[0005] The purpose of the present invention is to provide an adhesive for electronic precision devices and a preparation method thereof, wherein the adhesive cures quickly at room temperature, has good adhesion, is stable in storage, has good thermal conductivity, and can better meet the use requirements of electronic appliances.

[0006] To this end, the present invention adopts the following technical solutions:

[0007] The present invention provides an adhesive for electronic precision devices, comprising the following components in parts by weight:

[0008] 80-100 parts of naphthyl epoxy resin, 5-30 parts of siloxane, 5-25 parts of diluent, 10-50 parts of insulating thermal conductive material and 3-20 parts of composite curing agent;

[0009] The insulating thermal conductive material is an OH-BN / Al N / PLGA-PEG-NH2 composite material;

[0010] The composite curing agent comprises a modified polythiol curing agent A and a modified polythiol curing agent B, which are mixed in a mass ratio of (1-2.5):(1-2.5), and 0.05-1% of a silane coupling agent is added and stirred to obtain the composite curing agent.

[0011] Due to the rigid planar conjugated structure of the naphthalene ring, naphthalene-based epoxy resins have a series of excellent properties, such as low moisture absorption, high chemical resistance, low CTE and excellent mechanical and thermomechanical properties.

[0012] Furthermore, the method for preparing the insulating thermally conductive material comprises the following steps:

[0013] The preparation method of the OH-BN / AlN / PLGA-PEG-NH2 composite material comprises the following steps:

[0014] (1) Adding boron nitride to isopropanol and ultrasonically shaking in a water bath for 10-24 hours, adding NaOH solution and heating and stirring, the heating temperature is 110-150° C., the reaction time is 12-72 hours, filtering, washing with pure water 3-5 times, drying, and grinding to obtain hydroxyl-modified ON-BN powder;

[0015] (2) mixing OH-BN powder and aluminum nitride in a mass ratio of (0.5-1):(1-3), adding the mixture to a mixture of tris(hydroxymethylaminomethane) buffer and ethanol, ultrasonically dispersing for 20-30 min, stirring for reaction for 12-24 h, filtering, washing with ethanol 2-3 times, drying, and grinding to obtain OH-BN / AlN powder;

[0016] (3) adding OH-BN / AlN powder to chloroform, ultrasonicating for 24-48 hours, then removing the solvent and drying to obtain OH-BN / AlN flakes;

[0017] (4) dissolving the poly(lactic acid-co-glycolic acid) copolymer polyethylene glycol amino group in dichloromethane, adding the OH-BN / Al N sheet obtained in step (3), stirring and dispersing for 15-40 minutes, then pouring into a mold, removing the solvent, and demolding to obtain the OH-BN / Al N / PLGA-PEG-NH2 composite material.

[0018] Preferably, the concentration of the sodium hydroxide solution in step (1) is 50-150 g / L.

[0019] Preferably, the mass percentage of OH-BN / AlN in the OH-BN / AlN / PLGA-PEG-NH2 composite material of step (3) is 10-50%.

[0020] Furthermore, the preparation method of the modified polythiol curing agent A comprises: heating and stirring the reaction of glycerol triglycidyl ether and pentaerythritol tetrakis(3-mercaptopropionic acid) ester in a molar ratio of (1-3):1 under the action of a catalyst.

[0021] Preferably, the catalyst is triethylamine; and / or the heating reaction temperature is 60-80° C.; and / or the reaction time is 6-24 h.

[0022] Furthermore, the preparation method of the modified polythiol curing agent B comprises: heating and stirring the reaction of hexamethylene diisocyanate and pentaerythritol tetrakis(3-mercaptopropionic acid) in a molar ratio of (0.5-4):1 under the action of a catalyst.

[0023] Preferably, the catalyst is an organic tin catalyst, more preferably dibutyltin dilaurate; and / or the heating reaction temperature is 60-80° C.; and / or the reaction time is 6-24 h.

[0024] Preferably, the siloxane is selected from one or more of vinyl silane, amino silane, epoxy silane, mercapto silane and methacryloxy silane.

[0025] Preferably, the diluent is selected from one or more of alkylene glycidyl ether, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, benzyl glycidyl ether, and butyl glycidyl ether.

[0026] Preferably, the adhesive further comprises one or more of a toughening agent, a plasticizer, a defoaming agent, an antioxidant, and an antioxidant.

[0027] The present invention also provides a method for preparing an adhesive for electronic precision devices, comprising the following steps:

[0028] 1) After the naphthyl epoxy resin and the siloxane are blended and melted, a diluent is added and the mixture is stirred and mixed uniformly;

[0029] 2) adding an insulating thermally conductive material and a sulfur-containing curing agent for blending, with a curing temperature of 25-150° C. and a heating rate of 5-20° C. / min to obtain the adhesive for electronic precision devices.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The adhesive for electronic precision devices of the present invention is a composite curing agent obtained by mixing naphthyl epoxy resin, siloxane, a diluent, OH-BN / AlN / polylactic acid-hydroxyacetic acid copolymer polyethylene glycol amino composite thermal conductive insulating material, modified polythiol curing agent A and modified polythiol curing agent B. The composite curing agent has excellent bonding performance and thermal conductivity and fast curing speed at room temperature.

[0032] The insulating thermal conductive material OH-BN / Al N / PLGA-PEG-NH2 composite material provided by the present invention adopts nanosheets of edge hydroxylated boron nitride and aluminum nitride composite material to react with PLGA-PEG-NH2, and the nanosheets are uniformly dispersed and bonded on the long molecular chain of PLGA-PEG-NH2, which greatly increases the specific surface area of ​​the nanomaterial, and also significantly improves the dispersibility of boron nitride and aluminum nitride and the compatibility of the system. Adding them can better improve the performance of the material.

[0033] The composite curing agent provided by the present invention is a composite of a modified polythiol curing agent A and a modified polythiol curing agent B. After modification, more diverse functional groups are introduced, and at the same time, a good cross-linking structure is provided, so that the adhesive system can obtain a better network structure and enhance the bonding performance. The composite curing agent of the present invention realizes instant curing and has good storage stability.

[0034] The present invention adopts naphthalene epoxy resin as the base resin, and by melting and mixing with siloxane, the resin base has better reactivity and heat resistance, and is combined with the thermal conductive material and curing agent of the system to obtain good bonding force and thermal conductivity.

[0035] The adhesive provided by the invention has excellent comprehensive performance and has good application prospects in electronic devices. DETAILED DESCRIPTION

[0036] Below by specific embodiment, the specific implementation mode of this explanation technical scheme is further described, these embodiments are for the detailed description of this technical scheme, rather than for limiting this technical scheme. Based on the embodiment in this description, all other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the scope of protection of this description. Unless otherwise specified, the reagent, method and equipment used in the present invention are conventional reagents, methods and equipment in the art, and the reagents and materials used in the following examples are all commercially available.

[0037] Naphthalene epoxy resin EBA-65 was purchased from Hubei Langbowan Biopharmaceutical Co., Ltd.;

[0038] Hexagonal boron nitride was purchased from Shenzhen Advanced New Materials Manufacturing Co., Ltd.;

[0039] Aluminum nitride, CAS No. 24304-00-5, purchased from Hebei Teng Bimetallic Materials Co., Ltd.;

[0040] Poly(lactic acid-co-glycolic acid)-poly(ethylene glycol)-amino (PLGA-PEG-NH2), molecular weight 2000, was purchased from Xi'an Ruixi Biotechnology Co., Ltd.

[0041] Preparation Example 1

[0042] This preparation example provides a modified thiol curing agent A, and the preparation method is as follows: weigh 49g of pentaerythritol tetrakis(3-mercaptopropionic acid) ester and 1g of triethylamine and add them into a three-necked flask, stir mechanically, add 13g of propylene glycol triglycidyl ether dropwise into the three-necked flask, heat to 70°C, stir and react for 18h, and collect the product to obtain.

[0043] Preparation Example 2

[0044] This preparation example provides a modified thiol curing agent B, and the preparation method is as follows: weigh 85g of pentaerythritol tetrakis(3-mercaptopropionic acid) ester and dibutyltin dilaurate and add them into a three-necked flask, stir mechanically, drop 16.8g of toluene diisocyanate into the three-necked flask, react and stir at 65°C for 12h, collect the product, and obtain the product.

[0045] Preparation Example 3

[0046] Preparation of a composite curing agent: Mix the modified thiol curing agent A of Preparation Example 1 and the modified thiol curing agent B of Preparation Example 2 in a mass ratio of 1:1, add 0.3% of silane coupling agent Z-6040, and stir for 20 minutes to obtain a composite curing agent.

[0047] The composite curing agent is used in the following examples and comparative examples.

[0048] Preparation Example 4

[0049] This preparation example provides an insulating thermal conductive material OH-BN / Al N / PLGA-PEG-NH2 composite material, and its preparation method comprises the following steps:

[0050] (1) Add 20 g of boron nitride (BN) to 100 mL of isopropanol and ultrasonically vibrate in a water bath for 10-24 h, add 50 mL of a 120 g / L NaOH solution and heat with stirring at 140 ° C. The reaction time is 24 h, filter, wash with pure water 5 times, dry, and grind to obtain hydroxyl-modified ON-BN powder;

[0051] (2) OH-BN and aluminum nitride (AlN) were mixed in a mass ratio of 1:3, added to a mixture of tris(hydroxymethylaminomethane) buffer and ethanol, ultrasonically dispersed for 30 min, stirred for reaction for 20 h, filtered, washed with ethanol three times, dried, and ground to obtain OH-BN / AlN powder;

[0052] (3) adding the OH-BN / AlN powder prepared above into 150 mL of chloroform, ultrasonicating for 48 h, then removing the solvent, drying, and grinding to obtain OH-BN / AlN flakes;

[0053] (4) Dissolve polylactic acid-co-glycolic acid polyethylene glycol amino (PLGA-PEG-NH2) in dichloromethane, add the OH-BN / AlN sheet prepared in step (3) at a mass ratio of 50%, stir and disperse for 40 minutes, then pour into a mold, remove the solvent, and demold to obtain an OH-BN / AlN / PLGA-PEG-NH2 composite material.

[0054] Example 1

[0055] This embodiment provides an adhesive for electronic precision devices, comprising the following components in parts by weight:

[0056] 80 parts of naphthyl epoxy resin, 20 parts of siloxane KH560, 15 parts of 1,4-butanediol diglycidyl ether, 40 parts of insulating thermal conductive material and 10 parts of composite curing agent;

[0057] The insulating thermal conductive material is the OH-BN / Al N / PLGA-PEG-NH2 composite material prepared in Preparation Example 4;

[0058] The composite curing agent is the composite curing agent prepared in Preparation Example 3, and the composite curing agent is composite-prepared before preparing the adhesive.

[0059] The method for preparing an adhesive for electronic precision devices provided in this embodiment comprises the following steps:

[0060] 1) After the naphthyl epoxy resin and the siloxane are blended and melted, a diluent is added and the mixture is stirred and mixed uniformly;

[0061] 2) adding insulating thermal conductive material and composite curing agent for blending, dispersing by ultrasonic wave, and curing at a temperature of 25° C. to obtain the adhesive for electronic precision devices.

[0062] Example 2

[0063] This embodiment provides an adhesive for electronic precision devices, comprising the following components in parts by weight:

[0064] 100 parts of naphthyl epoxy resin, 10 parts of siloxane KH560, 15 parts of 1,4-butanediol diglycidyl ether, 40 parts of insulating thermal conductive material and 5 parts of polythiol curing agent;

[0065] The insulating thermal conductive material is the OH-BN / Al N / PLGA-PEG-NH2 composite material prepared in Preparation Example 4;

[0066] The composite curing agent is the composite curing agent prepared in Preparation Example 3, and the composite curing agent is composite-prepared before preparing the adhesive.

[0067] The method for preparing an adhesive for electronic precision devices provided in this embodiment comprises the following steps:

[0068] 1) After the naphthyl epoxy resin and the siloxane are blended and melted, a diluent is added and the mixture is stirred and mixed uniformly;

[0069] 2) adding insulating thermal conductive material and composite curing agent for blending, dispersing by ultrasonic wave, and curing at a temperature of 25° C. to obtain the adhesive for electronic precision devices.

[0070] Example 3

[0071] This embodiment provides an adhesive for electronic precision devices, comprising the following components in parts by weight:

[0072] 90 parts of naphthyl epoxy resin, 20 parts of siloxane KH560, 20 parts of benzyl glycidyl ether, 50 parts of insulating thermal conductive material and 15 parts of polythiol curing agent;

[0073] The insulating thermal conductive material is the OH-BN / Al N / PLGA-PEG-NH2 composite material prepared in Preparation Example 4;

[0074] The composite curing agent is the composite curing agent prepared in Preparation Example 3, and the composite curing agent is composite-prepared before preparing the adhesive.

[0075] The method for preparing an adhesive for electronic precision devices provided in this embodiment comprises the following steps:

[0076] 1) After the naphthyl epoxy resin and the siloxane are blended and melted, a diluent is added and the mixture is stirred and mixed uniformly;

[0077] 2) adding insulating thermal conductive material and composite curing agent for blending, dispersing by ultrasonic wave, and curing at a temperature of 25° C. to obtain the adhesive for electronic precision devices.

[0078] Comparative Example 1

[0079] Compared with Example 1, the difference is that the insulating thermal conductive material hydroxyl-modified BN / AlN / poly PLGA-PEG-NH2 composite material is replaced by BN in equal parts by weight, and the rest are the same.

[0080] The preparation method of the adhesive in this comparative example is the same as that in Example 1.

[0081] Comparative Example 2

[0082] Compared with Example 1, the difference is that the insulating thermal conductive material hydroxyl-modified BN / AlN / PLGA-PEG-NH2 composite material is replaced by an equal weight portion of AlN, and the rest are the same.

[0083] The preparation method of the adhesive in this comparative example is the same as that in Example 1.

[0084] Comparative Example 3

[0085] Compared with Example 1, the difference is that the insulating thermal conductive material hydroxyl-modified BN / AlN / PLGA-PEG-NH2 composite material is replaced by an equal weight portion of BN and AlN mixed filler, and the molar ratio of BN and AlN is kept the same as the ratio of the two in the hydroxyl-modified BN / AlN / polylactic acid-glycolic acid copolymer polyethylene glycol amino composite, and the other parts are the same.

[0086] The preparation method of the adhesive in this comparative example is the same as that in Example 1.

[0087] Comparative Example 4

[0088] Compared with Example 1, the difference is that the insulating thermal conductive material hydroxyl-modified BN / AlN / PLGA-PEG-NH2 composite material is not added, and the other parts are the same.

[0089] The preparation method of the adhesive in this comparative example is the same as that in Example 1.

[0090] Comparative Example 5

[0091] Compared with Example 1, the difference is that the composite curing agent is replaced by the conventional curing agent polyetheramine D400, and the other parts are the same.

[0092] The preparation method of the adhesive in this comparative example is the same as that in Example 1.

[0093] Comparative Example 6

[0094] Compared with Example 1, the difference is that the composite curing agent only contains modified thiol curing agent A, and the others are the same.

[0095] The preparation method of the adhesive in this comparative example is the same as that in Example 1.

[0096] Comparative Example 7

[0097] Compared with Example 1, the difference is that the composite curing agent only contains the modified thiol curing agent B, and the others are the same.

[0098] The preparation method of the adhesive in this comparative example is the same as that in Example 1.

[0099] Comparative Example 8

[0100] Compared with Example 1, the difference is that no siloxane is added, and the other aspects are the same.

[0101] The preparation method of the adhesive in this comparative example is the same as that in Example 1.

[0102] Performance test: The following performance tests were performed on the adhesives prepared in Examples 1-3 and Comparative Examples 1-8.

[0103] 1. Thermal conductivity: measured in accordance with GB / T2588-2008 standard;

[0104] 2. Volume resistivity: refer to GB / T15662-1995 for volume resistivity test, the humidity of the test environment is 85%;

[0105] 3. Shear strength: The shear strength of the adhesives prepared in Examples 1-3 and Comparative Examples 1-8 according to GB / T 7124-2008 in 3003Al-3003Al, PET-PET substrates.

[0106] 4. Curing time: record the time required for curing at room temperature 25°C.

[0107] The test results are shown in Table 1 and Table 2.

[0108] Table 1 Adhesion curing performance test results

[0109]

[0110]

[0111] Table 2 Insulation thermal conductivity test results

[0112]

[0113] It can be seen from the test data of Examples 1-3 and Comparative Examples 1-8 given in Table 1 and Table 2 that the adhesive provided by the present invention has excellent bonding ability to both aluminum and PET plastic materials, the thermal conductivity of the adhesive provided by the present invention can reach 9.05 W / m·K, which is significantly higher than the thermal conductivity of ordinary epoxy adhesives, and has good insulation ability, and the adhesive provided by the present invention has a fast curing speed and can be cured at room temperature in 18-25 minutes.

[0114] It can be seen from the test data of Example 1 and Comparative Examples 1-8 that:

[0115] The addition of the insulating thermally conductive material provided by the present invention can significantly and effectively improve the thermal conductivity of the adhesive, and has a better effect of enhancing thermal conductivity than conventional thermally conductive fillers BN and Al N. The insulating thermally conductive material provided by the present invention can also enhance the shear strength of the adhesive and improve the bonding performance to aluminum and plastic materials.

[0116] The addition of the composite curing agent provided by the present invention can significantly increase the curing speed of the adhesive, and has better enhanced curing performance than conventional amine curing agents. In addition, the composite curing agent provided by the present invention is more effective in increasing the curing speed of the adhesive than any single-component curing agent, indicating that the two can synergistically increase the curing speed and improve the bonding performance after mixing.

[0117] The adhesive provided by the present invention is scientifically matched with naphthyl epoxy resin, siloxane, thermal conductive materials, etc., and under the action of a composite curing agent, a system structure having both good rigidity and good network crosslinking degree is formed. The thermal conductive materials are uniformly dispersed and bonded on the molecular chains in the system, so that the adhesive obtains good thermal conductivity and mechanical properties.

[0118] The adhesive provided by the present invention has excellent thermal conductivity and bonding performance, fast curing speed, helps to achieve more excellent application effects in the field of electronic packaging, and has good application prospects.

[0119] Although the embodiments of the present description have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present description, the scope of which is defined by the appended claims and their equivalents.

Claims

1. An adhesive for electronic precision devices, characterized in that: The composition comprises the following components in parts by weight: 80-100 parts of naphthyl epoxy resin, 5-30 parts of siloxane, 5-25 parts of diluent, 10-50 parts of insulating thermal conductive material and 3-20 parts of composite curing agent; The insulating thermal conductive material is an OH-BN / AlN / PLGA-PEG-NH2 composite material; The composite curing agent comprises a modified polythiol curing agent A and a modified polythiol curing agent B, which are mixed in a mass ratio of (1-2.5):(1-2.5), and 0.05-1% of a silane coupling agent is added and stirred to obtain the composite curing agent.

2. The adhesive for electronic precision devices according to claim 1, characterized in that: The preparation method of the OH-BN / AlN / PLGA-PEG-NH2 composite material comprises the following steps: (1) Add boron nitride to isopropanol and ultrasonically vibrate in a water bath for 10-24 hours, add NaOH and heat and stir at a heating temperature of 110-150°C for a reaction time of 12-72 hours, filter, wash with pure water for 3-5 times, dry, and grind to obtain OH-BN powder; (2) Mixing hydroxy-modified OH-BN powder and aluminum nitride in a mass ratio of (0.5-1):(1-3), adding the mixture to a mixture of tris(hydroxymethylaminomethane) buffer and ethanol, ultrasonically dispersing for 20-30 minutes, stirring for reaction for 12-24 hours, filtering, washing with ethanol for 2-3 times, drying, and grinding to obtain OH-BN / AlN powder; (3) Adding OH-BN / AlN powder to chloroform, ultrasonicating for 24-48 hours, then removing the solvent and drying to obtain OH-BN / AlN flakes; (4) Dissolve the poly(lactic acid-co-glycolic acid) copolymer polyethylene glycol amino group in dichloromethane, add the OH-BN / AlN sheet obtained in step (3), stir and disperse for 15-40 minutes, then pour into a mold, remove the solvent, and demold to obtain an OH-BN / AlN / PLGA-PEG-NH2 composite material.

3. The adhesive for electronic precision devices according to claim 2, characterized in that: The molar concentration of the sodium hydroxide solution in step (1) is 1-3.

4. The adhesive for electronic precision devices according to claim 2, characterized in that: The mass percentage of OH-BN / AlN in the OH-BN / AlN / PLGA-PEG-NH2 composite material of step (4) is 10-50%.

5. The adhesive for electronic precision devices according to claim 1, characterized in that: The preparation method of the modified polythiol curing agent A comprises: heating and stirring the reaction of glycerol triglycidyl ether and pentaerythritol tetrakis(3-mercaptopropionic acid) in a molar ratio of (1-3):1 under the action of a catalyst to obtain the obtained product.

6. The adhesive for electronic precision devices according to claim 1, characterized in that: The preparation method of the modified polythiol curing agent B comprises: heating and stirring the reaction of hexamethylene diisocyanate and pentaerythritol tetrakis(3-mercaptopropionic acid) in a molar ratio of (0.5-4):1 under the action of a catalyst to obtain the obtained product.

7. The adhesive for electronic precision devices according to claim 1, characterized in that: The siloxane is selected from one or more of vinyl silane, amino silane, epoxy silane, mercapto silane and methacryloxy silane.

8. The adhesive for electronic precision devices according to claim 1, characterized in that: The diluent further comprises one or more of alkylene glycidyl ether, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, benzyl glycidyl ether, and butyl glycidyl ether.

9. The adhesive for electronic precision devices according to any one of claims 1 to 8, characterized in that: It also includes one or more of a toughening agent, a plasticizer, a defoaming agent, an antioxidant, and an antioxidant.

10. A method for preparing an adhesive for electronic precision devices according to any one of claims 1 to 9, characterized in that: The steps include: 1) After the naphthyl epoxy resin and siloxane are blended and melted, a diluent is added and stirred to mix evenly; 2) Add insulating thermal conductive material and sulfur-containing curing agent for blending, with a curing temperature of 25-150° C. and a heating rate of 5-20° C. / min to obtain the adhesive for electronic precision devices.

Citation Information

Patent Citations

  • High-power LED substrate heat conduction and insulation material and manufacturing method thereof

    CN104945820A

  • Thermal-conductivity insulating material with good thermal conducting property for LED substrate

    CN105038079A

  • High-temperature-resistant powder coating

    CN105505114A

  • Water-resistant epoxy resin for silicon rod cutting and preparation method thereof

    CN112625218A

  • Soluble microneedle matrix material as well as preparation method and application thereof

    CN114146050A

Cited By

  • Adhesive for electronic precision device and preparation method thereof

    CN120758212A

  • An adhesive for electronic precision devices and a method for preparing the same

    CN120758212B