Deep-drawing-resistant and high-temperature-resistant block structure polyurethane adhesive for lithium ion battery packaging and preparation method thereof
By designing a block structure polyurethane adhesive that is resistant to deep impregnation and high temperature, it uses branched liquid rubber polyols, polyethers, isocyanate blocked polyester and high molecular weight ultraviolet initiator to solve the problem of depth resistance in lithium-ion battery packaging materials. The problem of difficult to take into account both impulse and high temperature resistance has achieved a high-performance, safe and environmentally friendly adhesive.
Patent Information
- Application Number
- CN202411091380.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Polyurethane adhesives for existing lithium-ion batteries aluminum-plastic composite packaging materials are difficult to take into account the properties of deep-pull resistance and high-temperature resistance, and there is a contradictory relationship between the two.
Using a block structure polyurethane adhesive composed of branched liquid rubber polyol-polyether-branched liquid rubber polyol copolymer, isocyanate blocked high-temperature hydrolysis polyester polyol and high molecular weight ultraviolet initiator, through Specific molecular design and process steps are prepared to form a deep-drain-resistant adhesive that is resistant to high temperatures.
It has achieved high flexibility, high temperature resistance and safety of lithium-ion battery packaging materials, significantly improved peel strength and deep drawing depth, and is non-toxic and environmentally friendly. It is suitable for aluminum-plastic composite packaging of lithium-ion batteries.
Smart Images

Figure CN118931456A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyurethane adhesive and a preparation method thereof, in particular to a deep-drawing and high-temperature-resistant block-structure polyurethane adhesive for lithium-ion battery packaging and a preparation method thereof; and belongs to the technical field of new materials. Background Art
[0002] Polyurethane adhesives are generally composed of two basic units, namely diisocyanate, polyester diol or polyether diol. "Soft segment" and "hard segment" are usually used to describe the polyurethane structure, among which the polyester diol or polyether diol chain segment is called the soft segment, and the diisocyanate is called the hard segment. Since the main chain components of polyurethane have a wide range of sources and types, its molecular structure design is more flexible. In addition, the main chain molecules of polyurethane adhesives contain a large number of physical crosslinks composed of hydrogen bonds, which give polyurethane adhesives higher strength, modulus, bonding performance, high temperature resistance and simple molding process than traditional materials. Among them, the two-component reactive polyurethane dry composite adhesive with good flexibility and excellent deep drawing resistance has excellent composite strength for plastic / plastic and plastic / aluminum composite structures, and is especially suitable for aluminum-plastic composites for lithium-ion battery packaging.
[0003] The invention patent with application number 202010174304.5 discloses a polyurethane laminating adhesive for lithium-ion batteries, which is mainly composed of a compound of water-soluble anionic polyurethane and water-soluble cationic polyurethane, wherein the water-soluble anion is a mixture of diisocyanate, polyethylene polyol and a salt-forming agent, and the water-soluble cationic polyurethane is a mixture of diisocyanate, polyetherimide, vegetable oil-modified polyol and a salt-forming agent. The invention patent with application number 201810524575.1 discloses a reactive polyurethane hot melt adhesive for hemming of soft-package lithium-ion batteries, and the raw materials for preparation include polyester polyol, polyether polyol, tackifying resin, thermoplastic elastomer, diisocyanate, catalyst, antioxidant and stabilizer.
[0004] The aluminum-plastic composite packaging materials for lithium-ion batteries prepared with polyurethane adhesives not only require deep-drawing resistance, but also high-temperature resistance, otherwise they will be flammable and explosive due to poor safety. For polyurethane adhesives, deep-drawing resistance requires good flexibility, while high-temperature resistance requires high cross-linking density, but these two are contradictory. How to balance the contradiction between the two is the key to developing deep-drawing and high-temperature resistant block-structure polyurethane adhesives. Summary of the invention
[0005] In order to overcome the deficiencies of the prior art, the purpose of the present invention is to provide a deep-drawing and high-temperature-resistant block-structure polyurethane adhesive and a preparation method thereof, so as to solve the problem that it is difficult to balance deep-drawing and high-temperature resistance of the existing polyurethane adhesives used in lithium-ion battery aluminum-plastic composite packaging materials.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A deep-drawing and high-temperature-resistant block-structure polyurethane adhesive for lithium-ion battery packaging is prepared by uniformly mixing the following components in parts by weight:
[0008] 100 parts of branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer;
[0009] 3-5 parts of high molecular weight UV initiator;
[0010] 20-35 parts of isocyanate-terminated high temperature hydrolyzable polyester polyol;
[0011] The branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer is first prepared from liquid rubber diol to obtain branched liquid rubber polyol, and then polyether diol is reacted with polyisocyanate to obtain isocyanate-terminated polyether diol oligomer, and finally branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer is prepared; the high molecular weight ultraviolet light initiator is prepared by modifying a hydroxyl-containing low molecular weight ultraviolet light initiator; the isocyanate-terminated high temperature hydrolyzable polyester polyol is prepared by reacting polyisocyanate with high temperature hydrolyzable polyester polyol, and the high temperature hydrolyzable polyester polyol is prepared by esterification and dehydration reaction of aromatic dibasic acid and flexible polyol.
[0012] The present invention also discloses a method for preparing a deep-drawing and high-temperature-resistant block-structure polyurethane adhesive for lithium-ion battery packaging as described above, comprising the following steps:
[0013] S1. Preparation of branched liquid rubber polyol:
[0014] Add 100 parts by mass of liquid rubber diol into a reaction container, heat to 60-90° C., then drop isocyanate trimer at a -NCO / -OH substance ratio of 0.1-0.3 for 1-2 hours, and continue to keep warm for 1-3 hours after the isocyanate trimer is dripped to obtain a branched liquid rubber polyol;
[0015] S2, preparation of branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer:
[0016] Add 100 parts by mass of polyisocyanate into a reaction container, heat to 60-90° C., then add polyether diol dropwise at a -NCO / -OH substance ratio of 2 for 1-2 hours, and continue to keep warm for 1-3 hours after the polyether diol is dripped to obtain an isocyanate-terminated polyether diol oligomer;
[0017] Next, slowly dripping 100% of the amount of the remaining isocyanate substance obtained in step S1 above for 1-2 hours, and then continuing to heat and react for 3-5 hours after dripping is completed, and cooling to obtain a branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer;
[0018] S3, preparation of high molecular weight ultraviolet initiator:
[0019] Add 100 parts by mass of polyisocyanate into a reaction container, heat to 60-90° C., then add polyether diol dropwise at a -NCO / -OH substance ratio of 2 for 1-2 hours, and continue to keep warm for 1-3 hours after the polyether diol is dripped to obtain an isocyanate-terminated polyether diol oligomer;
[0020] Next, slowly add 100% of the amount of the remaining isocyanate substance into the hydroxyl-containing low molecular weight ultraviolet photoinitiator, continue to keep warm and react for 3-5 hours, and cool to obtain a high molecular weight ultraviolet photoinitiator;
[0021] S4, preparation of high temperature resistant hydrolyzed polyester polyol:
[0022] Add 100 parts by weight of aromatic dibasic acid and 80-90 parts by weight of flexible polyol into a reaction container, heat to 160-190° C., perform esterification dehydration reaction for 3-5 hours, then heat to 210-230° C., perform vacuum polycondensation reaction for 4-6 hours, and cool to room temperature to obtain high temperature resistant hydrolyzed polyester polyol;
[0023] S5. Preparation of isocyanate-terminated high temperature resistant hydrolyzable polyester polyol:
[0024] Add 100 parts by mass of polyisocyanate into a reaction container, heat to 60-90° C., then add dropwise the high temperature resistant hydrolyzable polyester polyol obtained in step S4 at a molar ratio of -NCO / -OH of 2, add dropwise for 1-2 hours, continue to keep warm for 3-5 hours after the addition is complete, and cool to obtain isocyanate-terminated high temperature resistant hydrolyzable polyester polyol;
[0025] S6. Preparation of deep-drawing and high-temperature resistant block structure polyurethane adhesive:
[0026] 100 parts by weight of the branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer prepared in the above step S2, 3-5 parts by weight of the high molecular weight ultraviolet light initiator prepared in the above step S3, and 20-35 parts by weight of the isocyanate-terminated high temperature resistant hydrolyzed polyester polyol prepared in the above step S5 are uniformly mixed to obtain a deep drawing resistant and high temperature resistant block structure polyurethane adhesive.
[0027] Preferably, the reaction vessel is a four-necked flask equipped with a stirring device, a thermometer and a condenser.
[0028] More preferably, the liquid rubber diol is one of liquid polybutadiene diol and liquid polyisoprene diol, preferably liquid polybutadiene diol.
[0029] More preferably, the aforementioned isocyanate trimer is one of isophorone diisocyanate trimer and hexamethylene diisocyanate trimer.
[0030] More preferably, the polyisocyanate is one of isophorone diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate.
[0031] Still further preferably, the polyether diol is one of polyoxypropylene diol, polyoxyethylene propylene diol and polytetrahydrofuran diol; and the molecular weight of the polyether diol is 4000-6000.
[0032] More preferably, the aromatic dibasic acid is a mixture of phthalic acid and isophthalic acid, and the mass ratio of phthalic acid to isophthalic acid is 100:50-150.
[0033] More preferably, the flexible polyol is one of diethylene glycol, triethylene glycol, tetraethylene glycol, isopentyl glycol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol, preferably 1,4-cyclohexanedimethanol.
[0034] Still further preferably, the aforementioned hydroxyl-containing low molecular weight UV photoinitiator is one of 2-hydroxy-2-methyl-1-phenyl-1-propanone (photoinitiator 1173), 1-hydroxy-cyclohexyl-phenyl ketone (photoinitiator 184), 1,1'-(methylenebis-4,1-phenylene)bis[2-hydroxy-2-methyl-1-propanone] (photoinitiator 127), and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator 2959).
[0035] The present invention is beneficial in that:
[0036] (1) Compared with the solvent-based polyurethane adhesives currently on the market, the deep-drawing and high-temperature resistant segmented polyurethane adhesive of the present invention does not contain organic solvents and has the advantages of being non-toxic, safe to use, and environmentally friendly;
[0037] (2) The adhesive of the present invention particularly considers the requirements of deep-drawing and high-temperature resistant block-structure polyurethane adhesive for lithium-ion battery aluminum-plastic composite packaging materials, and prepares a special "high-temperature hydrolyzed polyester-branched liquid rubber polyol-polyether-branched liquid rubber polyol-high-temperature hydrolyzed polyester" block-structure polyurethane chain segment through molecular design, thereby optimizing the water resistance, yellowing resistance, deep-drawing resistance and high-temperature resistance of the polyurethane adhesive;
[0038] (3) In the present invention, the polyether diol with a relatively high molecular weight can provide high flexibility, and the high temperature hydrolysis resistant polyester polyol can not only improve the high temperature hydrolysis resistance of the film, but also improve the adhesion to the substrate. In the material design, the polyether diol and the high temperature hydrolysis resistant polyester polyol are separated by branched liquid rubber polyol molecules, so that the two form a certain distance to avoid mutual interference and give full play to their respective strengths.
[0039] (4) More importantly, the self-made high molecular weight UV initiator used in the present invention can avoid low molecular weight residues, has good compatibility with the block structure polyurethane chain segment, has a synergistic effect, and at the same time causes the liquid rubber to undergo a cross-linking reaction under ultraviolet light, further improving the high temperature resistance, thereby making the polyurethane adhesive integrate the properties of safety, environmental protection, water resistance, yellowing resistance, deep drawing resistance, and high temperature resistance, and the peel strength and deep drawing depth are significantly improved compared with the prior art and the comparative example. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a picture of a deep-drawn sample (lithium-ion battery packaging) prepared with the adhesive prepared in Example 1 of the present invention after aging at 120° C. for 24 hours;
[0041] Figure 2 This is a picture of a deep-drawn sample (lithium-ion battery packaging) prepared with the adhesive prepared in Comparative Example 1 after aging at 120° C. for 24 hours. DETAILED DESCRIPTION
[0042] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0043] Example 1
[0044] (1) Preparation of branched liquid rubber polyol
[0045] 100 parts by mass of liquid polybutadiene diol were added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, heated to 60°C, and then 2.1 parts by mass of hexamethylene diisocyanate trimer were added dropwise for 2 hours. After the addition was completed, the reaction was continued at the temperature for 3 hours to obtain a branched liquid rubber polyol.
[0046] (2) Preparation of branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer
[0047] 100 parts by weight of isophorone diisocyanate was added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, and the mixture was heated to 60° C. 900 parts by weight of polyoxypropylene diol with a molecular weight of 4000 was added dropwise for 1 hour. After the addition was completed, the mixture was kept warm for 3 hours to obtain an isocyanate-terminated polyether diol oligomer.
[0048] Next, 900 parts by weight of the branched liquid rubber polyol prepared above was slowly added dropwise for 1 hour. After the addition was completed, the mixture was kept warm for reaction for 3 hours and cooled to obtain a branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer.
[0049] (3) Preparation of high molecular weight UV photoinitiator
[0050] 100 parts by weight of isophorone diisocyanate was added to a light-proof four-necked flask equipped with a stirring device, a thermometer and a condenser, and the mixture was heated to 60° C. 900 parts by weight of polyoxypropylene diol with a molecular weight of 4000 was added dropwise for 1 hour. After the addition was completed, the mixture was kept warm for reaction for 3 hours to obtain an isocyanate-terminated polyether diol oligomer. Subsequently, 74 parts by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone was slowly added, the reaction was continued for 3 hours, and the mixture was cooled to obtain a high molecular weight ultraviolet light initiator.
[0051] (4) Preparation of high temperature resistant hydrolyzed polyester polyols
[0052] Into a four-necked flask equipped with a stirring device, a thermometer and a condenser, 67 parts by mass of terephthalic acid, 33 parts by mass of isophthalic acid and 80 parts by mass of 1,4-cyclohexanedimethanol were added, heated to 160°C, and an esterification dehydration reaction was carried out for 5 hours. The temperature was then raised to 210°C, and a vacuum polycondensation reaction was carried out for 6 hours. The mixture was cooled to room temperature to obtain a high temperature resistant hydrolyzed polyester polyol.
[0053] (5) Preparation of isocyanate-terminated high temperature hydrolysis-resistant polyester polyols
[0054] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of isophorone diisocyanate was added and heated to 60°C, and 225 parts by mass of the above-prepared high-temperature resistant hydrolyzable polyester polyol was added dropwise for 1 hour. After the addition was completed, the reaction was continued by keeping the temperature for 5 hours, and the isocyanate-terminated high-temperature resistant hydrolyzable polyester polyol was obtained.
[0055] (6) Preparation of deep-drawing and high-temperature resistant block-structured polyurethane adhesive
[0056] 100 parts by mass of the branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer prepared above, 3 parts by mass of the high molecular weight ultraviolet light initiator prepared above, and 20 parts by mass of the isocyanate-terminated high temperature resistant hydrolyzed polyester polyol prepared above are mixed evenly to obtain a deep drawing resistant and high temperature resistant block structure polyurethane adhesive.
[0057] Example 2
[0058] (1) Preparation of branched liquid rubber polyols
[0059] 100 parts by weight of liquid polybutadiene diol was added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, and heated to 75° C. Then 7 parts by weight of isophorone diisocyanate trimer was added dropwise for 1.5 hours. After the addition was completed, the reaction was continued at the temperature for 2 hours to obtain a branched liquid rubber polyol.
[0060] (2) Preparation of branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer
[0061] 100 parts by weight of dicyclohexylmethane diisocyanate was added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, and the mixture was heated to 80° C. Then, 950 parts by weight of polyoxypropylene diol with a molecular weight of 5000 was added dropwise for 1.5 hours. After the addition was completed, the mixture was kept warm for 2 hours to obtain an isocyanate-terminated polyether diol oligomer.
[0062] Next, 760 parts by weight of the branched liquid rubber polyol prepared above was slowly added dropwise for 1.5 hours. After the addition was completed, the mixture was kept warm for 4 hours and cooled to obtain a branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer.
[0063] (3) Preparation of high molecular weight UV photoinitiator
[0064] 100 parts by weight of dicyclohexylmethane diisocyanate was added to a light-proof four-necked flask equipped with a stirring device, a thermometer and a condenser, and the mixture was heated to 80° C. 954 parts by weight of polyoxypropylene diol with a molecular weight of 5000 was added dropwise for 1.5 hours. After the addition was completed, the mixture was kept warm for 3 hours to obtain an isocyanate-terminated polyether diol oligomer.
[0065] Next, 78 parts by mass of 1-hydroxy-cyclohexyl-phenyl ketone were slowly added, the reaction was continued for 4 hours, and the mixture was cooled to obtain a high molecular weight ultraviolet light initiator.
[0066] (4) Preparation of high temperature resistant hydrolyzed polyester polyols
[0067] Into a four-necked flask equipped with a stirring device, a thermometer and a condenser, 50 parts by mass of terephthalic acid, 50 parts by mass of isophthalic acid and 85 parts by mass of 1,4-cyclohexanedimethanol were added, heated to 180°C, and esterification and dehydration reaction was carried out for 4 hours. The temperature was then raised to 220°C, and vacuum polycondensation reaction was carried out for 5 hours. The reaction was cooled to room temperature to obtain a high temperature resistant hydrolyzed polyester polyol.
[0068] (5) Preparation of isocyanate-terminated high temperature hydrolysis-resistant polyester polyols
[0069] Into a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of dicyclohexylmethane diisocyanate was added, heated to 80°C, and 286 parts by mass of the above-prepared high-temperature resistant hydrolyzable polyester polyol was added dropwise for 1.5 hours. After the addition was completed, the reaction was continued by keeping the temperature for 4 hours, and cooled to obtain an isocyanate-terminated high-temperature resistant hydrolyzable polyester polyol.
[0070] (6) Preparation of deep-drawing and high-temperature resistant block-structured polyurethane adhesive
[0071] 100 parts by mass of the branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer prepared above, 3-5 parts by mass of the high molecular weight ultraviolet initiator prepared above, and 30 parts by mass of the isocyanate-terminated high temperature resistant hydrolyzed polyester polyol prepared above are mixed uniformly to obtain a deep drawing resistant and high temperature resistant block structure polyurethane adhesive.
[0072] Example 3
[0073] (1) Preparation of branched liquid rubber polyol
[0074] 100 parts by mass of liquid polybutadiene diol were added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, and heated to 90° C. Then 6.3 parts by mass of hexamethylene diisocyanate trimer were added dropwise for 1 hour. After the addition was completed, the reaction was continued at the temperature for 1 hour to obtain a branched liquid rubber polyol.
[0075] (2) Preparation of branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer
[0076] 100 parts by weight of hexamethylene diisocyanate was added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, and the mixture was heated to 90° C. 1800 parts by weight of polyoxypropylene diol with a molecular weight of 6000 was added dropwise for 2 hours. After the addition was completed, the mixture was kept warm for 1 hour to obtain an isocyanate-terminated polyether diol oligomer.
[0077] Next, 600 parts by weight of the branched liquid rubber polyol prepared above was slowly added dropwise for 2 hours. After the addition was completed, the mixture was kept warm for reaction for 3 hours and cooled to obtain a branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer.
[0078] (3) Preparation of high molecular weight UV photoinitiator
[0079] 100 parts by weight of hexamethylene diisocyanate was added to a light-proof four-necked flask equipped with a stirring device, a thermometer and a condenser, and the mixture was heated to 90° C. 1786 parts by weight of polyoxypropylene diol with a molecular weight of 6000 was added dropwise for 2 hours. After the addition was completed, the mixture was kept warm for 1 hour to obtain an isocyanate-terminated polyether diol oligomer.
[0080] Next, 100 parts by weight of 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone was slowly added, and the reaction was continued for 3 hours. The mixture was cooled to obtain a high molecular weight ultraviolet light initiator.
[0081] (4) Preparation of high temperature resistant hydrolyzed polyester polyols
[0082] Into a four-necked flask equipped with a stirring device, a thermometer and a condenser, 40 parts by mass of terephthalic acid, 60 parts by mass of isophthalic acid and 90 parts by mass of 1,4-cyclohexanedimethanol were added, heated to 190°C, and an esterification dehydration reaction was carried out for 3 hours. The temperature was then raised to 230°C, and a vacuum polycondensation reaction was carried out for 4 hours. The reaction was cooled to room temperature to obtain a high temperature resistant hydrolyzed polyester polyol.
[0083] (5) Preparation of isocyanate-terminated high temperature hydrolysis-resistant polyester polyols
[0084] Into a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of hexamethylene diisocyanate was added, heated to 90°C, and 595 parts by mass of the above-prepared high-temperature resistant hydrolyzable polyester polyol was added dropwise for 2 hours. After the addition was completed, the reaction was continued by keeping the temperature for 3 hours, and cooled to obtain an isocyanate-terminated high-temperature resistant hydrolyzable polyester polyol.
[0085] (6) Preparation of deep-drawing and high-temperature resistant block-structured polyurethane adhesive
[0086] 100 parts by mass of the branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer prepared above, 5 parts by mass of the high molecular weight ultraviolet initiator prepared above, and 35 parts by mass of the isocyanate-terminated high temperature resistant hydrolyzed polyester polyol prepared above are mixed uniformly to obtain a deep drawing resistant and high temperature resistant block structure polyurethane adhesive.
[0087] Comparative Example 1
[0088] (1) Preparation of hydroxyl-terminated polyurethane
[0089] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of isophorone diisocyanate and 1 part by mass of triphenyl phosphate were added, heated to 60°C, 3603 parts by mass of polyoxypropylene diol with a molecular weight of 4000 were added dropwise for 1 hour, and after the addition was completed, the reaction was continued at a temperature of 3 hours, and then cooled to obtain a hydroxyl-terminated polyurethane.
[0090] (2) Preparation of isocyanate-terminated polyester polyols
[0091] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of isophorone diisocyanate was added and heated to 60°C, and 225 parts by mass of polyethylene adipate with a molecular weight of 1000 was added dropwise for 1 hour. After the addition was completed, the reaction was continued at a temperature of 5 hours, and the isocyanate-terminated polyester polyol was obtained by cooling.
[0092] (3) Preparation of polyurethane adhesive
[0093] 100 parts by mass of the above-prepared hydroxyl-terminated polyurethane and 20 parts by mass of the above-prepared isocyanate-terminated polyester polyol were uniformly mixed to prepare a polyurethane adhesive.
[0094] Comparative Example 2
[0095] (1) Preparation of branched liquid rubber polyol
[0096] 100 parts by mass of liquid rubber diol were added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, heated to 60°C, and then 2.1 parts by mass of hexamethylene diisocyanate trimer were added dropwise for 2 hours. After the addition was completed, the reaction was continued at the temperature for 3 hours to obtain a branched liquid rubber polyol.
[0097] (2) Preparation of branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer
[0098] 100 parts by weight of isophorone diisocyanate was added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, and the mixture was heated to 60° C. 900 parts by weight of polyoxypropylene diol with a molecular weight of 4000 was added dropwise for 1 hour. After the addition was completed, the mixture was kept warm for 3 hours to obtain an isocyanate-terminated polyether diol oligomer.
[0099] Next, 900 parts by weight of the branched liquid rubber polyol prepared above was slowly added dropwise for 1 hour. After the addition was completed, the mixture was kept warm for reaction for 3 hours and cooled to obtain a branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer.
[0100] (3) Preparation of high temperature resistant hydrolyzed polyester polyols
[0101] Into a four-necked flask equipped with a stirring device, a thermometer and a condenser, 67 parts by mass of terephthalic acid, 33 parts by mass of isophthalic acid and 80 parts by mass of 1,4-cyclohexanedimethanol were added, heated to 160°C, and an esterification dehydration reaction was carried out for 5 hours. The temperature was then raised to 210°C, and a vacuum polycondensation reaction was carried out for 6 hours. The mixture was cooled to room temperature to obtain a high temperature resistant hydrolyzed polyester polyol.
[0102] (4) Preparation of isocyanate-terminated high temperature hydrolysis-resistant polyester polyols
[0103] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of isophorone diisocyanate was added and heated to 60°C, and 225 parts by mass of the above-prepared high-temperature resistant hydrolyzable polyester polyol was added dropwise for 1 hour. After the addition was completed, the reaction was continued by keeping the temperature for 5 hours, and the isocyanate-terminated high-temperature resistant hydrolyzable polyester polyol was obtained.
[0104] (5) Preparation of polyurethane adhesive
[0105] 100 parts by mass of the branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer prepared above, 3 parts by mass of 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173) ultraviolet light initiator, and 20 parts by mass of the isocyanate-terminated high temperature resistant hydrolyzable polyester polyol prepared above are mixed uniformly to obtain the polyurethane adhesive of this comparative example.
[0106] Performance Testing
[0107] Preparation of peel strength test samples: The polyurethane adhesive was evenly coated on a 200mm×200mm nylon film, laminated with an aluminum foil of the same size, aged at 45±1℃ for 24 hours, and exposed to light with an intensity of 100mW / cm 2 , and then irradiated with ultraviolet light of wavelength 365nm for 30s and cut into 200mm×15mm peel strength test samples.
[0108] Preparation of deep drawing test samples: The polyurethane adhesive was evenly coated on a 200mm×200mm nylon film, laminated with an aluminum foil of the same size, aged at 45±1℃ for 24 hours, and exposed to light with an intensity of 100mW / cm 2 , and then irradiated with ultraviolet light of wavelength 365nm for 30s to obtain the deep drawing test sample.
[0109] 1. Yellowing resistance test
[0110] The polyurethane adhesive was evenly applied to a polytetrafluoroethylene plate, aged at 45±1℃ for 24 hours, and then exposed to light with an intensity of 100mW / cm 2 , irradiate with ultraviolet light of wavelength 365nm for 30s to obtain a film sample with a thickness of 0.1-0.2mm, irradiate under a 1KW ultraviolet lamp for 15 minutes, and measure according to GB / T1766-2008 standard.
[0111] 2. Peel strength at room temperature
[0112] According to the national standard GB / T 2791-1995, the peel strength was tested at 25±1℃ using a CMT microcomputer-controlled electronic universal tensile testing machine.
[0113] 3. Peel strength after boiling
[0114] According to the national standard GB / T 2791-1995, the peel strength was tested at 25±1℃ using a CMT microcomputer-controlled electronic universal tensile testing machine.
[0115] 4. High temperature peel strength
[0116] According to the national standard GB / T 2791-1995, the peel strength was tested at 100±1℃ using a CMT microcomputer-controlled electronic universal tensile testing machine.
[0117] 5. Peel strength after thermal aging
[0118] The peel strength test sample prepared above was heat aged at 120±1°C for 120 hours and then placed at 25±1°C for 24 hours. The peel strength was tested at 25±1°C using a CMT microcomputer-controlled electronic universal tensile testing machine according to the national standard GB / T 2791-1995.
[0119] 6. Peel strength after wet heat aging
[0120] The peel strength test sample prepared above was subjected to damp heat aging for 120 hours at a temperature of 85±1°C and a relative humidity of 85±5%, and then placed at 25±1°C for 24 hours, and then the peel strength was tested at 25±1°C using a CMT microcomputer-controlled electronic universal tensile testing machine according to the national standard GB / T 2791-1995.
[0121] 7. Deep drawing depth
[0122] The punching die is 80mm*40mm, the maximum depth is 20mm, and the impact pressure is 0.7MPa. If the shell is punched 20 times continuously at a certain depth, there is no tearing or damage of the aluminum filling or delamination of the aluminum-plastic film, which means that the nylon / aluminum foil bonding layer is qualified at this punching depth. The maximum qualified impact depth of each sample is taken and recorded as the deep drawing depth.
[0123] The test results of the products of Examples 1-3 and Comparative Examples 1-2 are shown in Table 1 below:
[0124]
[0125] Table 1
[0126] As can be seen from Table 1, after the adhesive is compounded and cured, the room temperature peel strength, high temperature peel strength, peel strength after heat aging, peel strength after wet heat aging, and deep drawing depth of Examples 1-3 are significantly improved compared with Comparative Examples 1-2. The applicant analyzed that this is because the specific structure polyurethane chain segment of "high temperature resistant hydrolyzed polyester-branched liquid rubber polyol-polyether-branched liquid rubber polyol-high temperature resistant hydrolyzed polyester" is prepared by molecular design, and the polyurethane chain segments of different structures play their own roles and have a synergistic effect. The high molecular weight ultraviolet light initiator can avoid low molecular weight residues and has good compatibility with the block structure polyurethane chain segment. At the same time, the liquid rubber undergoes a cross-linking reaction under ultraviolet light, further improving the high temperature resistance. The peel strength in each case is significantly improved, and the deep drawing depth reaches more than 8.8 mm.
[0127] In addition, in order to compare product performance more intuitively, Figure 1 and Figure 2 The pictures of deep-drawn samples (lithium-ion battery packaging) prepared by the adhesives of Example 1 and Comparative Example 1 after aging at 120°C for 24 hours after deep-drawing are presented respectively. It can be seen from the figure that the deep-drawn sample of Example 1 is intact, while the deep-drawn sample of Comparative Example 1 has very obvious wrinkles, bulges and cracks due to poor peel strength and aging resistance. It can be seen that the polyurethane adhesive of the present invention is more suitable for lithium-ion battery packaging, and the product has outstanding properties such as deep-drawing resistance and high temperature resistance.
[0128] In summary, the deep-drawing and high-temperature resistant segmented polyurethane adhesive produced by the present invention has excellent performance, good system compatibility, fast curing speed, high production efficiency, easy industrialization, and wide application. No toxic solvents are released during the entire process, and it is a non-toxic, pollution-free, and environmentally friendly adhesive.
[0129] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. A deep-drawing and high-temperature resistant block structure polyurethane adhesive for lithium-ion battery packaging, It is characterized in that The following components in parts by weight are mixed uniformly: 100 parts of branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer; 3-5 parts of high molecular weight UV initiator; 20-35 parts of isocyanate-terminated high temperature hydrolyzable polyester polyol; The branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer is first prepared from liquid rubber diol to obtain branched liquid rubber polyol, then polyether diol oligomers terminated with isocyanate are prepared, and finally branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer is prepared; The high molecular weight ultraviolet light initiator is prepared by modifying a hydroxyl-containing low molecular weight ultraviolet light initiator; The isocyanate-terminated high-temperature hydrolyzable polyester polyol is prepared by the reaction of polyisocyanate and high-temperature hydrolyzable polyester polyol, and the high-temperature hydrolyzable polyester polyol is prepared by the esterification and dehydration reaction of aromatic dibasic acid and flexible polyol.
2. A method for preparing a deep-drawing and high-temperature resistant block structure polyurethane adhesive for lithium-ion battery packaging as claimed in claim 1, It is characterized in that The steps include: S1. Preparation of branched liquid rubber polyol: Add 100 parts by mass of liquid rubber diol into a reaction container, heat to 60-90° C., then drop isocyanate trimer at a -NCO / -OH substance ratio of 0.1-0.3 for 1-2 hours, and continue to keep warm for 1-3 hours after the isocyanate trimer is dripped to obtain a branched liquid rubber polyol; S2, preparation of branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer: Add 100 parts by mass of polyisocyanate into a reaction container, heat to 60-90° C., then add polyether diol dropwise at a -NCO / -OH substance ratio of 2 for 1-2 hours, and continue to keep warm for 1-3 hours after the polyether diol is dripped to obtain an isocyanate-terminated polyether diol oligomer; Next, slowly dripping 100% of the amount of the remaining isocyanate substance obtained in step S1 above for 1-2 hours, and then continuing to heat and react for 3-5 hours after dripping is completed, and cooling to obtain a branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer; S3, preparation of high molecular weight ultraviolet initiator: Add 100 parts by mass of polyisocyanate into a reaction container, heat to 60-90° C., then add polyether diol dropwise at a -NCO / -OH substance ratio of 2 for 1-2 hours, and continue to keep warm for 1-3 hours after the polyether diol is dripped to obtain an isocyanate-terminated polyether diol oligomer; Next, slowly add 100% of the amount of the remaining isocyanate substance into the hydroxyl-containing low molecular weight ultraviolet photoinitiator, continue to keep warm and react for 3-5 hours, and cool to obtain a high molecular weight ultraviolet photoinitiator; S4, preparation of high temperature resistant hydrolyzed polyester polyol: Add 100 parts by weight of aromatic dibasic acid and 80-90 parts by weight of flexible polyol into a reaction container, heat to 160-190° C., perform esterification dehydration reaction for 3-5 hours, then heat to 210-230° C., perform vacuum polycondensation reaction for 4-6 hours, and cool to room temperature to obtain high temperature resistant hydrolyzed polyester polyol; S5. Preparation of isocyanate-terminated high temperature resistant hydrolyzable polyester polyol: Add 100 parts by mass of polyisocyanate into a reaction container, heat to 60-90° C., then add dropwise the high temperature resistant hydrolyzable polyester polyol obtained in step S4 at a molar ratio of -NCO / -OH of 2, add dropwise for 1-2 hours, continue to keep warm for 3-5 hours after the addition is complete, and cool to obtain isocyanate-terminated high temperature resistant hydrolyzable polyester polyol; S6. Preparation of deep-drawing and high-temperature resistant block structure polyurethane adhesive: 100 parts by weight of the branched liquid rubber polyol-polyether-branched liquid rubber polyol polyurethane copolymer prepared in step S2, 3-5 parts by weight of the high molecular weight ultraviolet initiator prepared in step S3, 20-35 parts by weight of the isocyanate-terminated high-temperature-resistant hydrolyzed polyester polyol prepared in S5 are mixed evenly to obtain a deep-drawing-resistant and high-temperature-resistant segmented polyurethane adhesive.
3. The method for preparing the deep-drawing and high-temperature-resistant block structure polyurethane adhesive for lithium-ion battery packaging according to claim 1, It is characterized in that The reaction container is a four-necked flask equipped with a stirring device, a thermometer and a condenser.
4. The method for preparing the deep-drawing and high-temperature-resistant block-structure polyurethane adhesive for lithium-ion battery packaging according to claim 1, It is characterized in that The liquid rubber diol is one of liquid polybutadiene diol and liquid polyisoprene diol.
5. The method for preparing the deep-drawing and high-temperature-resistant block-structure polyurethane adhesive for lithium-ion battery packaging according to claim 1, It is characterized in that The isocyanate trimer is one of isophorone diisocyanate trimer and hexamethylene diisocyanate trimer.
6. The deep-drawing and high-temperature-resistant segmented polyurethane adhesive according to claim 1, It is characterized in that The polyisocyanate is one of isophorone diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate.
7. The deep-drawing and high-temperature-resistant segmented polyurethane adhesive according to claim 1, It is characterized in that The polyether diol is one of polyoxypropylene diol, polyoxyethylene propylene diol and polytetrahydrofuran diol; the molecular weight of the polyether diol is 4000-6000.
8. The deep-drawing and high-temperature-resistant segmented polyurethane adhesive according to claim 1, It is characterized in that The aromatic dibasic acid is a mixture of phthalic acid and isophthalic acid, and the mass ratio of phthalic acid to isophthalic acid is 100:50-150.
9. The deep-drawing and high-temperature-resistant segmented polyurethane adhesive according to claim 1, It is characterized in that The flexible polyol is one of diethylene glycol, triethylene glycol, tetraethylene glycol, isopentyl glycol, 1,6-hexanediol and 1,4-cyclohexanedimethanol.
10. The deep-drawing and high-temperature-resistant segmented polyurethane adhesive according to claim 1, It is characterized in that The hydroxyl-containing low molecular weight ultraviolet light initiator is one of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxy-cyclohexyl-phenyl ketone, 1,1'-(methylenebis-4,1-phenylene)bis[2-hydroxy-2-methyl-1-propanone], and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.
Citation Information
Patent Citations
Reactive type polyurethane hot melt adhesive for flexible packaging lithium ion battery edgefold
CN108753235A
Preparation method of polyurethane laminating adhesive for lithium battery
CN111205805A
Preparation method of acid and alkali resistant ultraviolet-curing adhesive film resin for glass base material
CN104086742A
Preparation method of thermoplastic polyurethane-polystyrene block copolymer
CN104530335A
Preparation method of solvent-free double-component polyurethane cooking adhesive
CN107722917A