Room-temperature-cured dealcoholized organosilicon sealant as well as preparation method and application thereof
Through room temperature cured dealcoholized silicone sealant combined with alkoxy-terminated polysiloxane and other components, the problem of insufficient oil resistance and high and low temperature resistance in high and low temperatures in high and low temperatures is solved, and the problem of silicone rubber is insufficient in high and low temperature resistance in high and low temperatures is realized for automobiles and machinery Highly efficient sealing performance in the manufacturing field.
Patent Information
- Application Number
- CN202411237642.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When used in high temperature and oil, the existing silicone rubber has insufficient oil resistance and high and low temperature resistance, resulting in a decrease in the strength and mechanical properties of the sealant, which cannot meet the high temperature and oily environment needs in automobiles, mechanical manufacturing and other fields.
Develop a room-temperature cured dealcoholized silicone sealant, using alkoxy-terminated polysiloxane, diluent, thixotropic agent, filler, water removal agent, crosslinking agent, tackifier, oil-resistant additive, The combination of heat-resistant agent and catalyst forms a sealant with excellent oil resistance and high and low temperature resistance through specific mixing and heating treatment.
It achieves good adhesion and aging stability to metal and plastic substrates, especially excellent performance in high temperature and oily environments, meets the sealing needs in automobiles, machinery manufacturing and other fields, and improves the adhesion of sealants and Durability.
Smart Images

Figure BDA0005028215040000031 
Figure BDA0005028215040000121 
Figure BDA0005028215040000122
Abstract
Description
Technical Field
[0001] The invention relates to an organic silicon sealant, in particular to a room temperature curing dealcoholized organic silicon sealant and a preparation method and application thereof, belonging to the technical field of organic silicon materials. Background Art
[0002] Silicone rubber is a high molecular weight polysiloxane with Si-O-Si structure as the main body. It has excellent weather resistance, electrical insulation, radiation resistance, oxygen resistance, aging resistance, high and low temperature resistance, biological inertness and other characteristics, making it widely used in the fields of automobiles, electronics and electrical, home construction, medical food, artificial organs, etc.
[0003] Conventional silicone rubber can be used for a long time in the range of -60 to 200°C. Its disadvantage is that it has poor anti-swelling ability against non-polar solvents, fuel oil and mineral oil, especially hot oil. When immersed in hot oil, it will swell quickly and its mechanical properties will be greatly reduced. However, with the development of modern science and technology, in industrial production such as the automotive industry, machinery manufacturing, and oil extraction, it is necessary to keep in contact with fuel, lubricating oil, hydraulic oil and other oils. During use, oils can penetrate into the rubber, causing mutual diffusion between molecules, changing the network structure of the vulcanized rubber, and thus reducing the strength and other mechanical properties of the sealant. This puts higher requirements on the adhesion, heat resistance and oil resistance of the sealant. For example, the temperature of the engine compartment of a fuel engine can be sustained above 300°C, which puts higher requirements on oil resistance and high and low temperature resistance for each accessory.
[0004] In addition, for many industrial manufacturing fields such as automobile and machinery manufacturing, the oil products used are mainly divided into the following two categories: one is engine oil lubricant, the other is gear oil; engine oil lubricant is mainly used for lubrication between engine parts, and gear oil is mainly used for lubrication of gearboxes and gearboxes. Engine oil lubricant and gear oil have certain differences in terms of use conditions, composition and performance. The main chemical components of both oils include high-boiling point, high-molecular-weight hydrocarbons and non-hydrocarbon mixtures, which are generally composed of alkanes (straight chain, branched chain, multi-branched chain), cycloalkanes (single ring, double ring, multi-ring), aromatics (single ring aromatics, polycyclic aromatics), cycloalkyl aromatics, and oxygen-containing, nitrogen-containing, sulfur-containing organic compounds and non-hydrocarbon compounds such as colloids and asphaltene; and different additives are added according to different uses. The additives are mainly chemical substances such as acids, alkalis / lipids, such as sulfur-phosphorus or sulfur-phosphorus-nitrogen additives. These substances change themselves under high temperature conditions of 120-150℃, and also have a large corrosive effect on silicone rubber, destroying the bonding and bulk properties of silicone rubber, causing the seal to fail. In addition, the working environment is basically at high temperature, which causes the oil to cause double damage to the silicone rubber material itself and the interface bonding.
[0005] At present, the three leakage problems in the fields of automobile and machinery manufacturing are mainly solved by bonding and sealing the flange end faces. The de-oxime system silicone rubber is corrosive to metals and has certain environmental protection limitations. Although it has certain oil resistance and high and low temperature resistance, it does not meet the growing demand; and the existing dealcoholized silicone rubber cannot fully meet the oil resistance and high and low temperature resistance. Although some foreign brand products can meet the current demand, they are expensive and cannot meet the needs of technological development; other system products are not suitable for applications in these fields. These are problems that need to be solved urgently. Summary of the invention
[0006] In order to solve the above technical problems, the present invention first proposes a room temperature curing dealcoholized silicone sealant, which can be cured at room temperature, has good adhesion to metals and most plastic substrates, good aging stability, and especially has excellent oil resistance and high and low temperature resistance.
[0007] Secondly, the present invention also provides a method for preparing a room temperature curing dealcoholized organic silicon sealant, which is simple to operate and has good applicability.
[0008] Thirdly, the present invention also provides an application of a room temperature-curing dealcoholized silicone sealant in the field of industrial manufacturing; based on the application advantages of the silicone sealant of the present invention, it is particularly suitable for use as a sealant in the fields of automobiles and machinery manufacturing, and has the advantages of good adhesion, oil resistance, high and low temperature resistance, and aging resistance.
[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0010] A room temperature curing dealcoholized organic silicon sealant, comprising the following components by weight: 45-60 parts of alkoxy-terminated polysiloxane; 2-4 parts of diluent; 2-5 parts of thixotropic agent; 40-50 parts of filler; 1-5 parts of dehydrating agent; 1-5 parts of crosslinking agent; 1-2 parts of tackifier; 1-2 parts of oil-resistant additive; 2-4 parts of heat-resistant agent; 0.1-0.3 parts of catalyst; 0.5-1.5 parts of color additive;
[0011] The structural expression of the tackifier is shown in Formula I:
[0012]
[0013] Among them, m=3~5, n=2~5.
[0014] The tackifier described in Formula I of the present invention is synthesized with reference to the preparation method of the tackifier in Patent 202311797574.1. The structure of Formula I contains a large number of alkoxy groups, which can react with the hydroxyl groups on the surface of the substrate to enhance the bonding strength and improve the oil resistance stability of the product; the -NCOO- five-membered ring body in the structure can not only effectively improve the adhesion to various substrates, but also further improve the oil resistance and heat resistance stability of the product; the above structure is symmetrical as a whole, and its weight average molecular weight is larger than that of conventional tackifiers, so that it has better uniformity in the product and higher stability in use.
[0015] In some preferred embodiments, the viscosity of the alkoxy-terminated polysiloxane is 15000 to 35000 mPa.s;
[0016] Preferably, the alkoxy-terminated polysiloxane is selected from one or more of trimethoxy-terminated polysiloxane, triethoxy-terminated polysiloxane, and methyldimethoxy-terminated polysiloxane.
[0017] In some preferred embodiments, the diluent is a reactive diluent with a viscosity of 50 to 100 mPa.s, preferably alkoxy mono-terminated polysiloxane, more preferably one or more of trimethoxy mono-terminated polysiloxane and triethoxy mono-terminated polysiloxane.
[0018] The diluent selected in the present invention can reduce the viscosity of the system and retain a reactive group at one end, which can react to the main structure during curing, provide enhanced toughness, and ensure the stability of the product.
[0019] In some preferred embodiments, the thixotropic agent is one or more of hydrophobic fumed silica, precipitated silica, and diatomaceous earth;
[0020] Preferably, the filler is one or more of calcium carbonate powder and silicon powder with a D50 of 20 to 40 nanometers;
[0021] Preferably, the dehydrating agent is hexamethyldisilazane;
[0022] Preferably, the crosslinking agent is one or more of methyltrimethoxysilane, methyltriethoxysilane and vinyltrimethoxysilane.
[0023] In some preferred embodiments, the oil-resistant additive is polyoxypropylene oxyethylene glycerol ether, with a molecular weight of 1500 to 3000, an acid value of ≤0.5 mgKOH / g, and a pH value of 5.0 to 7.0.
[0024] The inventors have also unexpectedly discovered in their ongoing research that by using polyoxypropylene oxyethylene glycerol ether as an oil-resistant additive, the polyether molecules are filled between the polysiloxane molecular chains, which hinders the free rotation of the Si-O bonds and Si-C bonds in the siloxane main chain (-SiOSi-) around the axis, increases the steric hindrance, and prevents hot oil molecules from entering during the aging process to attack and destroy the siloxane molecular chains. This can synergistically improve the heat resistance and oil resistance of the sealant, thereby bringing about good thermal stability and resistance to corrosion by various oil products, thereby enhancing its application advantages.
[0025] In some preferred embodiments, the heat-resistant agent is one or both of cerium oxide and iron oxide;
[0026] Preferably, the catalyst is one or more of n-butyl titanate, tetraisopropyl titanate, TYZOR-9000, TYZOR-722, and TYZOR-726;
[0027] Preferably, the color auxiliary agent is a black paste.
[0028] The present invention also provides a method for preparing the room temperature curing dealcoholized organosilicon sealant as described above, comprising the following steps:
[0029] After the alkoxy-terminated polysiloxane, diluent, thixotropic agent, filler, oil-resistant additive, heat-resistant agent and color additive are uniformly mixed in a high-speed mixer, dewatering agent, crosslinking agent and tackifier are added and continued to mix, and finally the catalyst is added. After the mixing reaction, stirring is stopped and the material is discharged.
[0030] In the method for preparing the room temperature curing dealcoholized silicone sealant, the mixing parameters of the materials are, for example:
[0031] Add alkoxy-terminated polysiloxane, diluent, thixotropic agent, filler, oil-resistant additive, heat-resistant agent and color additive into the mixing container, set the speed of the high-speed stirrer: revolution 20-25rpm, high-speed dispersion 600-800rpm, mix for 20-40min, stop and scrape the wall; continue to set the speed of the high-speed stirrer: revolution 30-35rpm, high-speed dispersion 1000-1500rpm, turn on heating 115-125℃, mix for 30-60min; continue to set the speed of the high-speed stirrer: revolution 30-35rpm, high-speed dispersion 800-1000rpm, keep heating 115-125℃, turn on vacuum -0.95--0.98MPa, and mix for another 40-60min; continue to set high-speed stirring The speed of the machine is: revolution 15-25rpm, high-speed dispersion 400-600rpm, maintain vacuum -0.95-0.98MPa, and stop stirring when the temperature drops below 30°C; then add dehydrating agent, cross-linking agent, and tackifier, set the speed of the high-speed stirrer: revolution 20-30rpm, high-speed dispersion 600-800rpm, turn off vacuum, perform nitrogen protection, maintain the temperature at 30-35°C, and mix for 25-30min; then add catalyst, set the speed of the high-speed stirrer: revolution 20-30rpm, high-speed dispersion 600-800rpm, maintain the temperature at 30-35°C, start vacuum -0.95-0.98MPa, mix for 40-60min, stop stirring at that time, and seal the discharged material for storage.
[0032] The present invention also provides an application of the room temperature curing dealcoholized organosilicon sealant as described above in the field of industrial manufacturing.
[0033] The invention solves the problem that the existing dealcoholized silicone rubber system cannot meet the use requirements in the fields of automobiles, machinery manufacturing, etc. in terms of oil resistance and high and low temperature resistance, and has good bonding performance and good aging resistance. DETAILED DESCRIPTION
[0034] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.
[0035] Unless otherwise specified, the following raw materials are from commercially available products.
[0036] Thickener: The thickener was synthesized according to the method in Example 1 of Patent 202311797574.1 (wherein m=4, n=2);
[0037] Alkoxy-terminated polysiloxane J-200: trimethoxy-terminated polysiloxane, viscosity 20000mPa.s, Keqi polymer materials
[0038] Alkoxy-terminated polysiloxane F-40A: Methyldimethoxy-terminated polysiloxane, viscosity 35000mPa.s, Keqi polymer materials
[0039] Alkoxy-terminated polysiloxane TEA: triethoxy-terminated polysiloxane, viscosity 15000mPa.s, Shanghai Huiyan New Materials Co., Ltd.
[0040] Alkoxy mono-terminated polysiloxane MP-68: trimethoxy mono-terminated polysiloxane, viscosity 70mPa.s, Keqi polymer materials
[0041] Alkoxy mono-terminated polysiloxane ASS-3010: triethoxy mono-terminated polysiloxane, viscosity 100mPa.s, Yuyao Huihong Plastic Factory
[0042] Hydrophobic fumed silica R974: Evonik
[0043] Precipitated silica F-397: Jingjinda New Materials
[0044] Diatomaceous earth: Shijiazhuang Baijiang Mineral Products Co., Ltd., super white 600 mesh diatomaceous earth powder
[0045] Calcium carbonate powder: Hangzhou Jikang New Materials Co., Ltd., SS-CAC40, D50 is 40 nanometers
[0046] Silica powder: Shijiazhuang Baijiang Mineral Products Co., Ltd., ultra-white 600 mesh diatomaceous earth
[0047] Polyoxypropylene oxyethylene glycerol ether A: Jiangsu Hai'an Petrochemical Plant, GPE3000, molecular weight 3000, acid value ≤0.5mgKOH / g, pH value 5.0~7.0
[0048] Polyoxypropylene oxyethylene glycerol ether B: Jiangsu Hai'an Petrochemical Plant, PPE1500, molecular weight 1500, acid value ≤0.5mgKOH / g, pH value 5.0~7.0
[0049] Polyoxypropylene oxyethylene glycerol ether C: Jiangsu Hai'an Petrochemical Plant, BPE2500, molecular weight 2500, acid value ≤0.5mgKOH / g, pH value 5.0~7.0
[0050] Cerium Oxide: Qiming New Materials
[0051] Iron oxide: Wuhu Xinda New Material Technology Co., Ltd., iron oxide red, 500 mesh
[0052] Black paste 3801: Shanghai Jingyi Industrial Co., Ltd.
[0053] Hexamethyldisilazane BOSIL-999: Hubei New Blue Sky New Materials Co., Ltd.
[0054] Vinyltrimethoxysilane: Hangzhou Jessica Chemical Co., Ltd.
[0055] Methyltrimethoxysilane: Hangzhou Jessica Chemical Co., Ltd., KH-131
[0056] Methyltriethoxysilane: Hangzhou Jessica Chemical Co., Ltd., KH-132
[0057] Butyl Titanate: Merck Chemical Technology (Shanghai) Co., Ltd.
[0058] Tetraisopropyl titanate: Merck Chemical Technology (Shanghai) Co., Ltd.
[0059] TYZOR-9000: Guangzhou Jianyi Chemical
[0060] TYZOR-722: Guangzhou Jianyi Chemical
[0061] TYZOR-726: Guangzhou Jianyi Chemical
[0062] The main testing methods involved in the present invention are as follows:
[0063] (1) Shear strength: Select 2024-T3 aluminum sheets with a size of 10 mm*25 mm*2 mm, apply a 1 mm thick adhesive layer, and cure at 25°C / 50% RH for 21 days. According to ASTM D1002 standard, use a universal tensile machine with a tensile rate of 5 mm / min to measure the shear strength of the samples. The results are the average of 5 tests.
[0064] (2) Tensile strength and elongation at break: Samples were prepared and tested in accordance with GB / T 528-2009 “Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber”. The sample size in this patent was a dumbbell-shaped specimen of the national standard. A universal tensile testing machine was used at a tensile rate of 500 mm / min to measure the tensile strength and elongation at break of the sample. The results were taken as the average of three tests.
[0065] [Example 1]
[0066] Add 55g J-200, 3g MP-68, 3.5g R974, 45g calcium carbonate powder, 1.5g polyoxypropylene oxyethylene glycerol ether A, 3g cerium oxide, and 1g black paste 3801 into a mixing container, set the speed of the high-speed stirrer: revolution 25rpm, high-speed dispersion 800rpm, mix for 40min, stop and scrape the wall; continue to set the speed of the high-speed stirrer: revolution 35rpm, high-speed dispersion 1500rpm, turn on heating at 120℃, mix for 60min; continue to set the speed of the high-speed stirrer: revolution 35rpm, high-speed dispersion 1000rpm, keep heating at 120℃, turn on Vacuum -0.98MPa, and mix for another 60min; continue to set the speed of the high-speed stirrer: revolution 25rpm, high-speed dispersion 600rpm, maintain vacuum -0.98MPa, and stop stirring when the temperature drops to 30°C; add 3g hexamethyldisilazane BOSIL-999, 3g vinyltrimethoxysilane, and 1.5g tackifier, set the speed of the high-speed stirrer: revolution 30rpm, high-speed dispersion 800rpm, turn off vacuum, perform nitrogen protection, maintain the temperature at 35°C, and mix for 30min; add 0.3g TYZOR-9000, set the speed of the high-speed stirrer: revolution 30rpm, high-speed dispersion 800rpm, maintain the temperature at 35°C, start vacuum -0.98MPa, mix for 60min, stop stirring at that time, and seal the discharged material for storage.
[0067] [Example 2]
[0068] Add 45g F-40A, 4g ASS-3010, 2g F-397, 50g silica powder, 1g polyoxypropylene oxyethylene glycerol ether B, 2g iron oxide, and 1.5g black paste 3801 into a mixing container, set the speed of the high-speed mixer: revolution 20pm, high-speed dispersion 600rpm, mix for 20min, stop and scrape the wall; continue to set the speed of the high-speed mixer: revolution 30rpm, high-speed dispersion 1000rpm, turn on heating 125℃, mix for 30min; continue to set the speed of the high-speed mixer: revolution 30rpm, high-speed dispersion 800rpm, keep heating at 125℃, turn on Vacuum -0.95MPa, and mix for another 40min; continue to set the speed of the high-speed stirrer: revolution 15rpm, high-speed dispersion 400rpm, maintain vacuum -0.95MPa, and stop stirring when the temperature drops below 30°C; add 5g hexamethyldisilazane BOSIL-999, 5g methyltriethoxysilane, and 1g viscosity enhancer, set the speed of the high-speed stirrer: revolution 20rpm, high-speed dispersion 600rpm, turn off vacuum, perform nitrogen protection, maintain the temperature at 30°C, and mix for 25min; add 0.1g TYZOR-726, set the speed of the high-speed stirrer: revolution 20rpm, high-speed dispersion 600rpm, maintain the temperature at 30°C, start vacuum -0.95MPa, mix for 40min, stop stirring at that time, and seal the discharged material for storage.
[0069] [Example 3]
[0070] 60g TEA, 4g MP-68, 5g diatomaceous earth, 40g calcium carbonate powder, 2g polyoxypropylene oxyethylene glycerol ether C, 4g cerium oxide, and 0.5g black paste 3801 were added to a mixing container, and the speed of the high-speed mixer was set to: revolution 23pm, high-speed dispersion 700rpm, mixing for 30min, stopping to scrape the wall; the speed of the high-speed mixer was continued to be set to: revolution 32rpm, high-speed dispersion 1250rpm, heating at 115°C, and mixing for 45min; the speed of the high-speed mixer was continued to be set to: revolution 33rpm, high-speed dispersion 900rpm, heating at 115°C, vacuuming at -0.96MPa, and mixing for another 50min; the speed of the high-speed mixer was continued to be set to: revolution 33rpm, high-speed dispersion 900rpm, heating at 115°C, vacuuming at -0.96MPa, and mixing for another 50min; the speed of the high-speed mixer was continued to be set to: revolution 32rpm, high-speed dispersion 1250rpm, heating at 115°C, and mixing for 45min. Turn to 20rpm, high-speed dispersion 500rpm, maintain vacuum -0.96MPa, and stop stirring when the temperature drops to 30℃; then add 1g hexamethyldisilazane BOSIL-999, 1g methyltrimethoxysilane, 2g viscosity enhancer, set the speed of the high-speed stirrer: revolution 25rpm, high-speed dispersion 700rpm, turn off vacuum, perform nitrogen protection, maintain the temperature at 33℃, and mix for 27min; then add 0.2g n-butyl titanate, set the speed of the high-speed stirrer: revolution 25rpm, high-speed dispersion 700rpm, maintain the temperature at 33℃, start vacuum -0.96MPa, mix for 0min, stop stirring at that time, and seal the discharged material for storage.
[0071] [Example 4]
[0072] Add 50g J-200, 3g MP-68, 4g diatomaceous earth, 46g silicon powder, 1.3g polyoxypropylene oxyethylene glycerol ether B, 2.5g cerium oxide, and 0.8g black paste 3801 into a mixing container, set the speed of the high-speed stirrer: revolution 22rpm, high-speed dispersion 650rpm, mix for 25min, stop and scrape the wall; continue to set the speed of the high-speed stirrer: revolution 31rpm, high-speed dispersion 1100rpm, turn on heating 120℃, and mix for 40min; continue to set the speed of the high-speed stirrer: revolution 34rpm, high-speed dispersion 900rpm, keep heating at 125℃, turn on vacuum -0.98MPa, and mix for another 50min; continue to set the speed of the high-speed stirrer: revolution 22rpm, high-speed dispersion 550rpm, maintain vacuum -0.97MPa, and stop stirring when the temperature drops to 30℃; then add 2.5g hexamethyldisilazane BOSIL-999, 2g methyltrimethoxysilane, 1.5g viscosity enhancer, set the speed of the high-speed stirrer: revolution 20rpm, high-speed dispersion 650rpm, turn off vacuum, perform nitrogen protection, maintain the temperature at 32℃, and mix for 26min; then add 0.3g tetraisopropyl titanate, set the speed of the high-speed stirrer: revolution 28rpm, high-speed dispersion 700rpm, maintain the temperature at 35℃, start vacuum -0.98MPa, mix for 60min, stop stirring at that time, and seal the discharged material for storage.
[0073] [Example 5]
[0074] Add 55g F-40A, 3.5g ASS-3010, 3g R974, 43g calcium carbonate powder, 1.8g polyoxypropylene oxyethylene glycerol ether A, 3.5g iron oxide, and 1.4g black paste 3801 into a mixing container, set the speed of the high-speed stirrer: revolution 24rpm, high-speed dispersion 600rpm, mix for 35min, stop and scrape the wall; continue to set the speed of the high-speed stirrer: revolution 35rpm, high-speed dispersion 1400rpm, turn on heating 125℃, mix for 40min; continue to set the speed of the high-speed stirrer: revolution 30rpm, high-speed dispersion 800rpm, keep heating at 115℃, turn on Vacuum -0.98MPa, and mix for another 55min; continue to set the speed of the high-speed stirrer: revolution 25rpm, high-speed dispersion 450rpm, maintain vacuum -0.95MPa, and stop stirring when the temperature drops to 30°C; add 4.5g hexamethyldisilazane BOSIL-999, 4.5g methyltriethoxysilane, 1.8g viscosity enhancer, set the speed of the high-speed stirrer: revolution 23rpm, high-speed dispersion 800rpm, turn off vacuum, perform nitrogen protection, maintain the temperature at 30°C, and mix for 25min; add 0.15g TYZOR-722, set the speed of the high-speed stirrer: revolution 30rpm, high-speed dispersion 700rpm, maintain the temperature at 30°C, start vacuum -0.98MPa, mix for 50min, stop stirring at that time, and seal the discharged material for storage.
[0075] [Comparative Example 1]
[0076] The organic silicone sealant was prepared according to the same formula and method as in Example 3, except that the tackifier was replaced with KH560 of the same mass.
[0077] [Comparative Example 2]
[0078] The organosilicon sealant was prepared according to the same formula and method as in Example 3, except that no polyoxypropylene oxyethylene glycerol ether was added.
[0079] [Comparative Example 3]
[0080] Henkel Loctite 5970 was used as the silicone sealant.
[0081] [Comparative Example 4]
[0082] Henkel Loctite 5900 was used as the silicone sealant (deoxime system).
[0083] The performance of each sealant in each embodiment and comparative example was tested as shown in Table 1 and Table 2, and the results are as follows:
[0084] Table 1
[0085]
[0086] Table 2
[0087]
[0088] Damage status description:
[0089] Cohesive failure refers to the phenomenon that the adhesive layer itself breaks, separates or peels off. When peeling failure occurs in the sealant itself, it indicates that the bonding strength between the sealant and the bonded material is greater than the strength of the sealant itself.
[0090] Interface failure refers to the damage that occurs at the interface between the sealant and the bonded material, indicating that the bonding strength is less than the strength of the sealant itself.
[0091] Mixed failure refers to a mixture of interface failure and cohesive failure, that is, there is both partial interface failure and partial cohesive failure.
[0092] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.
Claims
1. A room temperature curing dealcoholized silicone sealant, characterized in that: The following components are included by weight: 45-60 parts of alkoxy-terminated polysiloxane; 2-4 parts of diluent; 2-5 parts of thixotropic agent; 40-50 parts of filler; 1-5 parts of dewatering agent; 1-5 parts of crosslinking agent; 1-2 parts of tackifier; 1-2 parts of oil-resistant additive; 2-4 parts of heat-resistant agent; 0.1-0.3 parts of catalyst; 0.5-1.5 parts of color additive; The structural expression of the tackifier is shown in Formula I: Among them, m=3~5, n=2~5.
2. The room temperature curing dealcoholized organosilicon sealant according to claim 1, characterized in that: The viscosity of the alkoxy-terminated polysiloxane is 15000 to 35000 mPa.s; Preferably, the alkoxy-terminated polysiloxane is selected from one or more of trimethoxy-terminated polysiloxane, triethoxy-terminated polysiloxane, and methyldimethoxy-terminated polysiloxane.
3. The room temperature curing dealcoholized organosilicon sealant according to claim 2, characterized in that: The diluent is a reactive diluent with a viscosity of 50 to 100 mPa.s, preferably alkoxy mono-terminated polysiloxane, more preferably one or more of trimethoxy mono-terminated polysiloxane and triethoxy mono-terminated polysiloxane.
4. The room temperature curing dealcoholized organosilicon sealant according to any one of claims 1 to 3, characterized in that: The thixotropic agent is one or more of hydrophobic fumed silica, precipitated silica, and diatomaceous earth; Preferably, the filler is one or more of calcium carbonate powder and silicon powder with a D50 of 20 to 40 nanometers; Preferably, the dehydrating agent is hexamethyldisilazane; Preferably, the crosslinking agent is one or more of methyltrimethoxysilane, methyltriethoxysilane and vinyltrimethoxysilane.
5. The room temperature curing dealcoholized organosilicon sealant according to any one of claims 1 to 4, characterized in that: The oil-resistant additive is polyoxypropylene oxyethylene glycerol ether, with a molecular weight of 1500-3000, an acid value of ≤0.5 mgKOH / g, and a pH value of 5.0-7.
0.
6. The room temperature curing dealcoholized organosilicon sealant according to any one of claims 1 to 5, characterized in that: The heat-resistant agent is one or both of cerium oxide and iron oxide; Preferably, the catalyst is one or more of n-butyl titanate, tetraisopropyl titanate, TYZOR-9000, TYZOR-722, and TYZOR-726; Preferably, the color auxiliary agent is a black paste.
7. A method for preparing a room temperature curing dealcoholized organosilicon sealant as claimed in any one of claims 1 to 6, characterized in that: The process includes: After the alkoxy-terminated polysiloxane, diluent, thixotropic agent, filler, oil-resistant additive, heat-resistant agent and color additive are uniformly mixed in a high-speed mixer, dewatering agent, crosslinking agent and tackifier are added and continued to mix, and finally the catalyst is added. After the mixing reaction, stirring is stopped and the material is discharged.
8. Use of the room temperature curing dealcoholized organosilicon sealant as claimed in any one of claims 1 to 6 in the field of industrial manufacturing.