Preparation method of hot-melt pressure-sensitive adhesive and application of hot-melt pressure-sensitive adhesive in rubber plaster
Through the preparation method of hot melt pressure sensitive adhesive, the problems of long production cycles and flammable and explosive in the existing technology are solved, the adhesion and safety of rubber paste are improved, and an efficient and environmentally friendly production process is achieved. It is suitable for Multiple medical uses.
Patent Information
- Application Number
- CN202410982754.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing hot melt pressure-sensitive adhesives have a long production cycle and low efficiency, and there is a risk of flammability and explosiveness during the preparation process, which affects drug safety and environmental pollution.
A new hot melt pressure-sensitive adhesive is prepared by mixing a specific proportion of thermoplastic elastomer TPE, softener, filler and tackifier, heat to a molten state and stirring, and then preparing a new hot melt pressure-sensitive adhesive, and applying it to the rubber paste, through Ethanol reflux extract and mixer stir to form a high-quality rubber paste.
It improves the adhesion and safety of rubber paste, reduces drug safety risks, reduces environmental pollution, ensures production safety, and is easy to use, does not contaminate clothing, and is suitable for the treatment of wounds and rheumatism and other diseases.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of traditional Chinese medicine pharmaceutical preparation, and particularly relates to a preparation method of a hot-melt pressure-sensitive adhesive and application of the hot-melt pressure-sensitive adhesive in a rubber patch. Background Art
[0002] Hot melt pressure sensitive adhesive is a type of pressure sensitive adhesive. It is a new type of adhesive tape made by mixing synthetic rubber, resin and rubber oil, heating them into a molten state, and then coating them on substrates such as cotton paper, cloth or plastic film. Its biggest advantage is its low cost, but its disadvantage is that its viscosity is significantly affected by temperature. It is mainly used for various types of sealing boxes, paper packaging, beverage bottle labels, sealing aluminum foil, waterproof coils, express delivery labels, flexible packaging and other packaging and environmentally friendly paper pallets, etc., and is suitable for various materials.
[0003] Thermoplastic rubber, also known as thermoplastic elastomer TPE, is a type of polymer material that has both rubber elasticity and plastic plasticity. It is also an environmentally friendly material that meets the needs of green and environmentally friendly development.
[0004] Rubber paste refers to an external dosage form in which drugs or medicinal material extracts are mixed with a rubber-based matrix and applied to the backing material. Rubber pastes are divided into ointments, plasters and patches. Ointments refer to semi-solid external preparations that are easily applied to the skin, mucous membranes or wounds by adding drugs to a suitable matrix. Plasters are external preparations that use edible vegetable oils and lead pastes made from high-temperature refined lead pastes such as yellow lead or lead powder as a matrix and contain drugs or Chinese medicinal material extracts. There are many types of plasters. The black plaster is based on oil and yellow lead; the white plaster is based on oil and palace powder; and the rosin plaster is based on rosin.
[0005] Rubber patch refers to a patch made by mixing raw material drugs with a matrix such as rubber and then coating it on a backing material. Summary of the invention
[0006] The purpose of the present invention is to solve the problems existing in the prior art such as long production cycle, low production efficiency, and flammable and explosive risks in the preparation process, and to provide a method for preparing a hot-melt pressure-sensitive adhesive and its application in a rubber patch, with the goal of improving the quality of the rubber patch, reducing the safety risk of drugs, reducing environmental pollution, and ensuring safe production.
[0007] In order to solve the problems of the prior art, the technical solution adopted by the present invention is:
[0008] A method for preparing a hot melt pressure-sensitive adhesive comprises the following steps:
[0009] Step 1: weigh 20-70 parts of thermoplastic elastomer TPE, 15-80 parts of softener, 3-15 parts of filler, and 20-70 parts of tackifier according to the mass ratio;
[0010] Step 2: After nitrogen is introduced into the reactor to exhaust the oxygen, softener, filler and viscosity enhancer are added and mixed and stirred for 20-60 minutes.
[0011] Heat to molten state at 110-130℃;
[0012] Step 3: Add thermoplastic elastomer TPE and continue stirring at 120-150°C for 1-3 hours. When the mixture forms a uniform, transparent, viscous liquid, discharge the mixture and cool it to obtain a hot melt pressure-sensitive adhesive.
[0013] Preferably, the softener is vaseline and / or liquid paraffin.
[0014] Preferably, the ratio of vaseline to liquid paraffin is 1:2.
[0015] Preferably, the tackifier is one or more of rosin, terpene resin, C5 petroleum resin, and hydrogenated petroleum resin.
[0016] Preferably, the filler is one or more of zinc oxide, calomel and lithopone.
[0017] The present application also discloses the use of the hot melt pressure sensitive adhesive prepared by any of the above preparation methods in a rubber patch, comprising the following steps:
[0018] Step 1: weigh 10-30 parts of the drug components of black-banded snake, 5-15 parts of raw croton, 30-50 parts of raw strychnine, 30-50 parts of angelica dahurica, 30-50 parts of mustard, 30-50 parts of earthworm, 30-50 parts of peach kernel, 30-50 parts of mandrake seeds, 30-50 parts of notopterygium, 10-30 parts of raw Chuanwu, 10-30 parts of raw arisaema, 30-50 parts of safflower, 30-50 parts of ephedra, 30-50 parts of siler, 30-50 parts of angelica, 30-50 parts of cinnamon, 15-20 parts of camphor, 15-20 parts of borneol, 40-50 parts of turpentine, 50-60 parts of methyl salicylate and 10-30 parts of menthol;
[0019] Step 2: mix 10-30 parts of jasper, 5-15 parts of raw croton, 30-50 parts of raw strychnine, 30-50 parts of angelica dahurica, 10-30 parts of raw aconite, 30-50 parts of angelica dahurica, 5-15 parts of mustard seeds, 30-50 parts of earthworm, 30-50 parts of peach kernel, 30-50 parts of mandrake seeds, 30-50 parts of notopterygium, 10-30 parts of raw aconite, 10-30 parts of raw arisaema, 30-50 parts of safflower, 30-50 parts of ephedra, 30-50 parts of siler, 30-50 parts of angelica, and 30-50 parts of cinnamon, and then reflux and extract with ethanol;
[0020] Step 3: Set the mixer temperature to 50-80°C, add the hot melt pressure sensitive adhesive, and after the hot melt pressure sensitive adhesive is melted, add the ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol into the mixer for mixing, stir thoroughly for 15-30 minutes, and then apply to the backing;
[0021] Step 4: After cooling, cover with an anti-sticking layer and then cut into pieces to obtain a rubber patch.
[0022] Preferably, the ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol constitute the drug component in the rubber patch, and the weight ratio of drug component: hot melt pressure-sensitive adhesive is 2-50:80-100.
[0023] Beneficial effects:
[0024] Compared with the prior art, the preparation method of a hot melt pressure-sensitive adhesive and the application thereof in a rubber patch of the present invention have the following advantages:
[0025] 1. This application develops a new matrix and a preparation process to improve the quality of Zhenjiang rubber paste, reduce drug safety risks, reduce environmental pollution, and ensure safe production;
[0026] 2. The product of the present invention has the advantages of strong adhesion, no need to heat and soften when in use, easy to use and carry, no contamination of clothes, etc.; it can protect wounds, prevent skin cracking, and treat rheumatism and other diseases;
[0027] 3. Change the natural rubber in the Zhenjiang rubber paste matrix into thermoplastic rubber, and add softener vaseline, liquid paraffin, tackifier rosin, and filler zinc oxide. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below through specific embodiments, but is not limited thereto.
[0029] Example 1
[0030] A method for preparing a hot melt pressure-sensitive adhesive comprises the following steps:
[0031] Step 1: weigh 20 parts of thermoplastic elastomer TPE, 5 parts of softener vaseline, 10 parts of softener liquid paraffin, 3 parts of filler zinc oxide, and 20 parts of tackifier rosin according to the mass ratio;
[0032] Step 2: After nitrogen is introduced into the reactor to exhaust oxygen, softener, filler and tackifier are added and mixed for 20 minutes, and heated at 110°C until they are molten;
[0033] Step 3: Add thermoplastic elastomer TPE and continue stirring at 120°C for 1 hour. When the mixture forms a uniform, transparent viscous liquid, discharge the mixture and cool it to obtain a hot melt pressure-sensitive adhesive.
[0034] An application of a hot melt pressure-sensitive adhesive in a rubber patch comprises the following steps:
[0035] Step 1: weigh the drug components 10 parts of black-banded snake, 5 parts of raw croton, 30 parts of raw strychnos nux vomica, 30 parts of angelica dahurica, 30 parts of mustard, 30 parts of earthworm, 30 parts of peach kernel, 30 parts of mandrake seeds, 30 parts of notopterygium, 10 parts of raw Chuanwu, 10 parts of raw arisaema, 30 parts of safflower, 30 parts of ephedra, 30 parts of siler, 30 parts of angelica, 30 parts of cinnamon, 15 parts of camphor, 15 parts of borneol, 40 parts of turpentine, 50 parts of methyl salicylate and 10 parts of menthol;
[0036] Step 2: 10 parts of black-banded snake, 5 parts of raw croton, 30 parts of raw strychnine, 30 parts of angelica dahurica, 10 parts of raw aconite, 30 parts of angelica dahurica, 5 parts of mustard seeds, 30 parts of earthworm, 30 parts of peach kernel, 30 parts of mandrake seeds, 30 parts of notopterygium, 10 parts of raw Chuanwu, 10 parts of raw arisaema, 30 parts of safflower, 30 parts of ephedra, 30 parts of siler, 30 parts of angelica, and 30 parts of cinnamon are mixed evenly and then extracted with ethanol by reflux;
[0037] Step 3: The kneading machine temperature is set to 50°C, and the hot melt pressure sensitive adhesive is added. After the hot melt pressure sensitive adhesive is melted, the ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol are all put into the mixer for mixing, and the mixture is fully stirred for 15 minutes and then coated on the backing;
[0038] Step 4: After cooling, cover with an anti-sticking layer and then cut into pieces to obtain a rubber patch.
[0039] The ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol constitute the drug component in the rubber patch, and the weight ratio of drug component: hot melt pressure-sensitive adhesive is 20:80.
[0040] Example 2
[0041] A method for preparing a hot melt pressure-sensitive adhesive comprises the following steps:
[0042] Step 1: weigh 70 parts of thermoplastic elastomer TPE, 40 parts of softener vaseline, 40 parts of softener liquid paraffin, 15 parts of filler zinc oxide, and 70 parts of tackifier rosin according to the mass ratio;
[0043] Step 2: After nitrogen is introduced into the reactor to exhaust oxygen, softener, filler and tackifier are added and mixed for 60 minutes, and heated at 130°C until they are molten;
[0044] Step 3: Add thermoplastic elastomer TPE and continue stirring at 150°C for 3 hours. When the mixture forms a uniform, transparent viscous liquid, discharge the mixture and cool it to obtain a hot melt pressure-sensitive adhesive.
[0045] An application of a hot melt pressure-sensitive adhesive in a rubber patch comprises the following steps:
[0046] Step 1: weigh 30 parts of drug components of black-banded snake, 15 parts of raw croton, 50 parts of raw strychnine, 50 parts of angelica dahurica, 30 parts of raw aconite, 50 parts of angelica dahurica, 15 parts of mustard, 50 parts of earthworm, 50 parts of peach kernel, 50 parts of mandsura seeds, 50 parts of notopterygium, 30 parts of raw Chuanwu, 30 parts of raw arisaema, 50 parts of safflower, 50 parts of ephedra, 50 parts of siler, 50 parts of angelica, 50 parts of cinnamon, 20 parts of camphor, 20 parts of borneol, 50 parts of turpentine, 60 parts of methyl salicylate and 30 parts of menthol according to the mass ratio;
[0047] Step 2: 30 parts of jasper, 15 parts of raw croton, 50 parts of raw strychnine, 50 parts of angelica dahurica, 30 parts of raw aconite, 50 parts of angelica dahurica, 15 parts of mustard seeds, 50 parts of earthworm, 50 parts of peach kernel, 50 parts of mandrake seeds, 50 parts of notopterygium, 30 parts of raw Chuanwu, 30 parts of raw arisaema, 50 parts of safflower, 50 parts of ephedra, 50 parts of siler, 50 parts of angelica, and 50 parts of cinnamon are mixed evenly and then extracted with ethanol by reflux;
[0048] Step 3: The kneading machine temperature is set at 80°C, and the hot melt pressure sensitive adhesive is added. After the hot melt pressure sensitive adhesive is melted, the ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol are all put into the mixer for mixing, and the mixture is fully stirred for 30 minutes and then coated on the backing;
[0049] Step 4: After cooling, cover with an anti-sticking layer and then cut into pieces to obtain a rubber patch.
[0050] The ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol constitute the drug component in the rubber patch, and the weight ratio of drug component: hot melt pressure-sensitive adhesive is 50:100.
[0051] Example 3
[0052] A method for preparing a hot melt pressure-sensitive adhesive comprises the following steps:
[0053] Step 1: weigh 50 parts of thermoplastic elastomer TPE, 20 parts of softener vaseline, 20 parts of softener liquid paraffin, 10 parts of filler zinc oxide, and 50 parts of tackifier rosin according to the mass ratio;
[0054] Step 2: After nitrogen is introduced into the reactor to exhaust oxygen, softener, filler and tackifier are added and mixed for 40 minutes.
[0055] Heat at 120°C until molten;
[0056] Step 3: Add thermoplastic elastomer TPE and continue stirring at 140°C for 2 hours. When the mixture forms a uniform, transparent viscous liquid, discharge the mixture and cool it to obtain a hot melt pressure-sensitive adhesive.
[0057] An application of a hot melt pressure-sensitive adhesive in a rubber patch comprises the following steps:
[0058] Step 1: weigh 20 parts of the drug components of black-banded snake, 10 parts of raw croton, 40 parts of raw strychnine, 40 parts of angelica dahurica, 40 parts of mustard, 40 parts of earthworm, 40 parts of peach kernel, 40 parts of mandrake seeds, 40 parts of notopterygium, 20 parts of raw Chuanwu, 20 parts of raw arisaema, 40 parts of safflower, 40 parts of ephedra, 40 parts of siler, 40 parts of angelica, 40 parts of cinnamon, 17 parts of camphor, 17 parts of borneol, 44 parts of turpentine, 54 parts of methyl salicylate and 20 parts of menthol according to the mass ratio;
[0059] Step 2: 20 parts of jasper, 10 parts of raw croton, 40 parts of raw strychnine, 40 parts of angelica dahurica, 40 parts of mustard seeds, 40 parts of earthworm, 40 parts of peach kernel, 40 parts of mandrake seeds, 40 parts of notopterygium, 20 parts of raw aconite, 20 parts of raw arisaema, 40 parts of safflower, 40 parts of ephedra, 40 parts of siler, 40 parts of angelica, and 40 parts of cinnamon are mixed evenly and then extracted with ethanol by reflux;
[0060] Step 3: The kneading machine temperature is set at 70°C, and the hot melt pressure sensitive adhesive is added. After the hot melt pressure sensitive adhesive is melted, the ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol are all put into the mixer for mixing, and the mixture is fully stirred for 20 minutes and then coated on the backing;
[0061] Step 4: After cooling, cover with an anti-sticking layer and then cut into pieces to obtain a rubber patch.
[0062] The ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol constitute the drug component in the rubber patch, and the weight ratio of drug component: hot melt pressure-sensitive adhesive is 40:90.
[0063] The embodiments described above are some embodiments of the present invention, rather than all embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed, but merely represents selected embodiments of the present invention.
[0064] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
Claims
1. A method for preparing a hot melt pressure-sensitive adhesive, characterized in that: The specific steps include: Step 1: weigh 20-70 parts of thermoplastic elastomer TPE, 15-80 parts of softener, 3-15 parts of filler, and 20-70 parts of tackifier according to the mass ratio; Step 2: After nitrogen is introduced into the reactor to exhaust oxygen, softener, filler and tackifier are added and mixed and stirred for 20-60 minutes, and heated at 110-130°C until they are molten; Step 3: Add thermoplastic elastomer TPE and continue stirring at 120-150°C for 1-3 hours. When the mixture forms a uniform, transparent, viscous liquid, discharge the mixture and cool it to obtain a hot melt pressure-sensitive adhesive.
2. The method for preparing a hot melt pressure sensitive adhesive according to claim 1, characterized in that: The softener is vaseline and / or liquid paraffin.
3. The method for preparing a hot melt pressure sensitive adhesive according to claim 2, characterized in that: The usage ratio of vaseline to liquid paraffin is 1:1-2.
4. The method for preparing a hot melt pressure sensitive adhesive according to claim 1, characterized in that: The tackifier is one or more of rosin, terpene resin, C5 petroleum resin, and hydrogenated petroleum resin.
5. The method for preparing a hot melt pressure sensitive adhesive according to claim 1, characterized in that: The filler is one or more of zinc oxide, calomel and lithopone.
6. Use of the hot melt pressure sensitive adhesive prepared by the preparation method according to any one of claims 1 to 5 in a rubber patch, characterized in that: The following steps are involved: Step 1: weigh 10-30 parts of the drug components of black-banded snake, 5-15 parts of raw croton, 30-50 parts of raw strychnine, 30-50 parts of angelica dahurica, 30-50 parts of mustard, 30-50 parts of earthworm, 30-50 parts of peach kernel, 30-50 parts of mandrake seeds, 30-50 parts of notopterygium, 10-30 parts of raw Chuanwu, 10-30 parts of raw arisaema, 30-50 parts of safflower, 30-50 parts of ephedra, 30-50 parts of siler, 30-50 parts of angelica, 30-50 parts of cinnamon, 15-20 parts of camphor, 15-20 parts of borneol, 40-50 parts of turpentine, 50-60 parts of methyl salicylate and 10-30 parts of menthol; Step 2: mix 10-30 parts of jasper, 5-15 parts of raw croton, 30-50 parts of raw strychnine, 30-50 parts of angelica dahurica, 10-30 parts of raw aconite, 30-50 parts of angelica dahurica, 5-15 parts of mustard seeds, 30-50 parts of earthworm, 30-50 parts of peach kernel, 30-50 parts of mandrake seeds, 30-50 parts of notopterygium, 10-30 parts of raw aconite, 10-30 parts of raw arisaema, 30-50 parts of safflower, 30-50 parts of ephedra, 30-50 parts of siler, 30-50 parts of angelica, and 30-50 parts of cinnamon, and then reflux and extract with ethanol; Step 3: Set the mixer temperature to 50-80°C, add the hot melt pressure sensitive adhesive, and after the hot melt pressure sensitive adhesive is melted, add the ethanol reflux extract, camphor, borneol, turpentine, methyl salicylate and menthol into the mixer for mixing, stir thoroughly for 15-30 minutes, and then apply to the backing; Step 4: After cooling, cover with an anti-sticking layer and then cut into pieces to obtain a rubber patch.