High-stability multi-element eutectic molten salt as well as preparation method and application thereof
By preparing high-stability multivariate eutectic molten salts containing NaNO3, NaNO2, Na2CO3, and KNO2, the problems of easy decomposition of nitrate molten salts at high temperatures and rising costs are solved, and molten salts with high stability and high specific heat capacity are achieved. In a variety of thermal energy applications.
Patent Information
- Application Number
- CN202411413700.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-12
AI Technical Summary
The existing nitrate molten salt is easily decomposed above 500 ℃, releasing harmful gases, resulting in the deterioration of thermal physical properties such as melting point, thermal decomposition temperature, specific heat, etc., and the cost is increasing year by year, increasing the cost of electric heating, and adding certain components. It will cause increased corrosion.
Provide a high stability multivariate eutectic molten salt containing 32.0~56.0wt.% NaNO3, 40.0~60.0wt.% NaNO2, 0~10.0%wt. Na2CO3, 0~13.0wt.% KNO2, and drying , grinding, mixing and muffle furnace melting treatment are prepared to form eutectic molten salts to improve stability and reduce costs.
The high-stability multi-eutectic eutectic molten salt is achieved while ensuring the thermal decomposition temperature and corrosion resistance, and the high-stability multi-eutectic molten salt formed has a minimum eutectic point of 180.0 ℃, the decomposition temperature can reach up to 678.5 ℃, and the average liquid specific heat is about 1.81. J/(g•K), suitable for solar photothermal power generation and other fields.
Smart Images

Figure CN118931505A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of solar thermal power generation technology, and in particular to a high-stability multi-element eutectic molten salt and a preparation method and application thereof. Background Art
[0002] Molten salts are widely used as heat transfer fluids in solar thermal power generation systems because of their excellent heat transfer and storage properties and low price. Among them, chloride salts are considered to be the most promising high-temperature heat transfer and storage medium due to their high natural abundance, low cost and good high-temperature stability. However, chloride salts are very corrosive to materials, which has become the main obstacle to their widespread application. Carbonates are widely used in chemical production and fuel cells, but because the melting points of single-component and two-component carbonates are usually higher than 500 °C, they are rarely used in heat transfer and storage materials.
[0003] Nitrates have unique advantages in terms of thermophysical properties, corrosion resistance and cost. Currently, the most widely used and mature nitrate molten salt in commercial applications at home and abroad is Solar salt (40wt.% KNO 3 -60wt.%NaNO 3 ) and Hitecsalt (53wt.%KNO 3 -7wt.%NaNO 3 -40wt.%NaNO 2 ), their operating temperature ranges are 300~565 ℃ and 200~535 ℃, and their specific heat capacities are 1.55 J / g•K and 1.54 J / g•K, respectively.
[0004] However, studies have shown that nitrates are prone to decomposition above 500°C, releasing NO x The harmful gases such as nitrate and nitrate molten salt decompose the melting point, thermal decomposition temperature, specific heat, viscosity and other thermal physical properties of the molten salt, thereby shortening the service life of the molten salt. To solve this problem, the research hotspot in recent years is to add other component salts to nitrate molten salts of different components to lower the melting point and increase the thermal decomposition temperature. For example, Chinese invention patent CN103074040B mentions adding Ca(NO 3 ) 2 -KNO 3 -NaNO 3 -NaNO 2 NaNO 2 Replaced by LiNO 3 The melting point of molten salt is about 50 ℃ lower than before; Chinese invention patent CN104479646B mentions that KNO 3 -Ca(NO 3 ) 2 -NaNO 2Add NaHPO 4 and Na 2 CO 3 The melting point of the molten salt is less than 140 °C, and the working temperature range is 140-550 °C. However, adding LiNO 3 Will significantly increase the cost of molten salt, Ca(NO 3 ) 2 The addition of nitrates and nitrites will cause the molten salt to easily absorb water, thus exacerbating corrosion. In addition, with the application of nitrates and nitrites in actual industry, their costs are also increasing year by year. Therefore, how to reduce the melting point and reduce the cost of electric heating while ensuring the thermal decomposition temperature and corrosion resistance is a key issue that needs to be solved at present. Summary of the invention
[0005] In view of the defects in the prior art, the object of the present invention is to provide a high-stability multi-element eutectic molten salt, which reduces the cost while ensuring the thermal decomposition temperature and corrosion resistance; in addition, the present invention also provides a preparation method and application of the high-stability multi-element eutectic molten salt.
[0006] The first aspect of the present invention provides a high-stability multi-component eutectic molten salt, wherein the high-stability multi-component eutectic molten salt comprises a single-component salt having the following weight percentage content: 32.0-56.0wt.% NaNO 3 、40.0~60.0wt.% NaNO 2 、0~10.0%wt.Na 2 CO 3 、0~13.0wt.% KNO 2 .
[0007] In one embodiment, the high stability multi-component eutectic molten salt is composed of single component salts with the following weight percentages: 40.0-56.0 wt.% NaNO 3 、44.0-60.0 wt.% NaNO 2 .
[0008] In one embodiment, the high stability multi-component eutectic molten salt is composed of single component salts with the following weight percentages: 35.0-55.0 wt.% NaNO 3 、43.0~58.0 wt.% NaNO 2 、1.0~10.0 wt.% Na 2 CO 3 .
[0009] In one embodiment, the high stability multi-element eutectic molten salt is composed of single component salts with the following weight percentages: 35.0-52.0 wt.% NaNO 3、40.0~55.0wt.% NaNO 2 、1.0~13.0wt.% KNO 2 .
[0010] In one embodiment, the high stability multi-element eutectic molten salt is composed of single component salts with the following weight percentages: 32.0-52.0 wt.% NaNO 3 、42.0~60.0wt.% NaNO 2 、1.0~10.0wt.% Na 2 CO 3 、1.0~13.0wt.%KNO 2 .
[0011] The second aspect of the present invention provides a method for preparing the above-mentioned high-stability multi-element eutectic molten salt, comprising the following steps: S1, drying the single-component salt raw materials separately; S2. Weigh the single-component salt in the formula, grind, and mix evenly to obtain a mixed salt; S3, placing the mixed salt in a muffle furnace to melt to obtain a molten salt, cooling the molten salt to room temperature, and grinding to obtain a high-stability multi-element eutectic molten salt; The temperature rise program of the muffle furnace is as follows: from room temperature to 100-120 °C, constant temperature for 12-24 h, and a heating rate of 5-10 K / min; from 100-120 °C to 300-450 °C, constant temperature for 12-24 h, and a heating rate of 5-10 K / min.
[0012] The third aspect of the present invention provides the application of the above-mentioned high-stability multi-element eutectic molten salt as a heat transfer / heat storage medium in the fields of solar thermal power generation, compressed air energy storage, industrial waste heat recovery, molten salt heat pump heat storage, off-peak electric thermal storage heating, and flexibility transformation of thermal power plants.
[0013] Compared with the prior art, the embodiments of the present invention have the following beneficial effects: 1. The high-stability multi-component eutectic molten salt provided by the present invention includes binary, ternary and quaternary molten salts, all of which form eutectic molten salts. The eutectic molten salt itself will inhibit decomposition and improve stability.
[0014] 2. The high-stability multi-component eutectic molten salt provided by the present invention has better overall thermophysical properties than non-eutectic molten salts with the same components.
[0015] 3. The high-stability multi-element eutectic molten salt provided by the present invention has a minimum eutectic point of 180.0°C and a decomposition temperature of up to 678.5°C. It has high stability, a wide temperature range, and high energy utilization.
[0016] 4. The high-stability multi-element eutectic molten salt provided by the present invention has an average specific heat of about 1.81 J / (g•K) in liquid state, which is greater than the specific heat of solar salt and Hitec salt, and has a high energy storage density.
[0017] 5. The high-stability multi-element eutectic molten salt provided by the present invention can be used as a heat transfer / heat storage medium in the fields of solar thermal power generation, compressed air energy storage, industrial waste heat recovery, molten salt heat pump heat storage, off-peak electric thermal storage heating, and flexibility transformation of thermal power plants. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings: Figure 1 This is the DSC curve of the high-stability multi-element eutectic molten salt in Example 1 of the present invention; Figure 2 TG curve of the high stability multi-element eutectic molten salt in Example 1 of the present invention; Figure 3 The specific heat curve of the liquid phase of the high-stability multi-element eutectic molten salt in Example 1 of the present invention; Figure 4 This is the DSC curve of the multi-component non-eutectic molten salt in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0019] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0020] Example 1 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1.
[0021] Table 1 Examples 1-24 and Comparative Examples 1-5
[0022] This embodiment also provides a method for preparing the above-mentioned high-stability multi-element eutectic molten salt, comprising the following steps: S1, drying the single-component salt raw materials separately; S2. Weigh the single-component salt in the formula, grind, and mix evenly to obtain a mixed salt; S3, placing the mixed salt in a muffle furnace to melt to obtain a molten salt, cooling the molten salt to room temperature, and grinding to obtain a high-stability multi-element eutectic molten salt; The temperature rise program of the muffle furnace is as follows: from room temperature to 100-120 °C, constant temperature for 12-24 h, and a heating rate of 5-10 K / min; from 100-120 °C to 300-450 °C, constant temperature for 12-24 h, and a heating rate of 5-10 K / min.
[0023] This embodiment and the following embodiments are all tested by the following steps: S1, NaNO 3 、NaNO 2 、KNO 2 、Na 2 CO 3 The four single-component salts were placed in a clean, dry container, dried at 120 °C in a drying oven for 12 h, and then cooled for later use; S2. After calibrating the electronic balance, accurately weigh NaNO according to the mass ratio in Table 1. 3 、NaNO 2 、KNO 2 、Na 2 CO 3 The four single-component salts were ground and mixed thoroughly in an agate mortar to obtain a mixed salt; S3. Transfer the obtained mixed salt to an alumina crucible that has been cleaned, dried and calcined in advance, cover the crucible and place it in a muffle furnace; set the temperature rising program of the muffle furnace as follows: from room temperature to 120 °C, keep the temperature constant for 6 h, and the heating rate is 10 K / min; from 120 °C to 300 °C, keep the temperature constant for 6 h, and the heating rate is 10 K / min; before the end of the program, pour the molten salt into a clean stainless steel basin, grind it after natural cooling, and bag it.
[0024] This embodiment also provides the application of high-stability multi-element eutectic molten salt as a heat transfer / heat storage medium in the fields of solar thermal power generation, compressed air energy storage, industrial waste heat recovery, molten salt heat pump heat storage, off-peak electric thermal storage heating, and flexibility transformation of thermal power plants.
[0025] Example 2 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0026] Example 3 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0027] Example 4 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0028] Example 5 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0029] Example 6 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0030] Example 7 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0031] Example 8 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0032] Example 9 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0033] Example 10 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0034] Embodiment 11 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0035] Example 12 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0036] Example 13 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0037] Embodiment 14 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0038] Embodiment 15 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0039] Example 16 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0040] Embodiment 17 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0041] Embodiment 18 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0042] Embodiment 19 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0043] Embodiment 20 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0044] Embodiment 21 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0045] Embodiment 22 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0046] Embodiment 23 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0047] Embodiment 24 This embodiment provides a high-stability multi-component eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the high-stability multi-component eutectic molten salt provided in this embodiment is the same as that in Example 1.
[0048] Comparative Example 1 This comparative example provides a multicomponent non-eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the multicomponent molten salt provided in this example is the same as that in Example 1.
[0049] Comparative Example 2 This comparative example provides a multicomponent non-eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the multicomponent molten salt provided in this example is the same as that in Example 1.
[0050] Comparative Example 3 This comparative example provides a multicomponent non-eutectic molten salt, and the composition and content of the single-component salt are shown in Table 1. The preparation method of the multicomponent molten salt provided in this example is the same as that in Example 1.
[0051] Comparative Example 4 This comparative example is Solar Salt eutectic molten salt, and the composition and content of the single component salt are shown in Table 1. The preparation method of the multicomponent eutectic molten salt provided in this example is the same as that in Example 1.
[0052] Comparative Example 5 This comparative example is Hitec Salt eutectic molten salt, and the composition and content of the single component salt are shown in Table 1. The preparation method of the multicomponent eutectic molten salt provided in this example is the same as that in Example 1.
[0053] Experimental example In this experimental example, the melting point, specific heat capacity, and decomposition temperature of the multi-element eutectic molten salt obtained in Examples 1-24 and Comparative Examples 1-5 were tested, and the results are shown in Table 2. The specific test method is as follows: The melting point of the prepared multi-component molten salt was tested by differential scanning calorimetry (DSC). The upper limit of the test temperature was 500 °C, the heating rate during the test was 10 K / min, an alumina crucible was selected as the container, and high-purity nitrogen was used as the protective gas. The presence of eutectic was determined by whether the melting peak in the DSC curve was a single peak. If there was no secondary peak, it was a eutectic salt, otherwise it was a non-eutectic salt.
[0054] The specific heat capacity of the prepared multi-component molten salt was tested by differential scanning calorimetry (DSC). The upper limit of the test temperature was 550°C, the heating rate during the test was 10 K / min, an alumina crucible was selected as the container, and high-purity nitrogen was used as the protective gas. The sample to be tested with a mass similar to that of the standard sample was accurately weighed and placed in the test crucible. The test was carried out using the same heating program as the baseline test and the standard sample test, and its specific heat capacity was obtained by calculation.
[0055] The thermal stability of molten salt was measured by synchronous thermal analyzer (TG-DSC). During the thermogravimetric test, a graphite crucible was selected as the container and high-purity nitrogen was used as the protective gas. 5-10 mg of molten salt sample was accurately weighed and placed in a graphite crucible, and the sample was heated to the target temperature at a heating rate of 10 K / min. Finally, the intersection of the baseline and the tangent of the inflection point of the loss weight curve was taken as the thermal decomposition temperature.
[0056] Table 2 Test results of multi-element eutectic molten salts obtained in Examples 1-24 and Comparative Examples 1-5 serial number Is it eutectic? Melting point(℃) Average specific heat of liquid phase (J / g∙K) Decomposition temperature(℃) Example 1 yes 182.3 1.81 678.5 Example 2 yes 180.5 1.88 662.0 Example 3 yes 180.0 1.88 660.8 Example 4 yes 180.8 1.87 662.6 Example 5 yes 183.0 1.89 660.5 Example 6 yes 182.3 1.87 665.5 Example 7 yes 181.2 1.91 648.0 Example 8 yes 206.4 1.93 645.6 Example 9 yes 227.5 1.84 668.2 Example 10 yes 186.6 1.80 673.3 Embodiment 11 yes 221.5 1.94 660.8 Example 12 yes 232.3 1.94 661.5 Example 13 yes 233.0 1.85 670.0 Embodiment 14 yes 221.8 1.94 661.3 Embodiment 15 yes 233.0 1.85 677.5 Example 16 yes 232.0 1.88 673.0 Embodiment 17 yes 215.5 1.93 623.8 Embodiment 18 yes 218.8 1.91 635.0 Embodiment 19 yes 218.5 1.91 651.0 Embodiment 20 yes 216.9 1.93 623.0 Embodiment 21 yes 229.5 1.95 581.8 Embodiment 22 yes 218.0 1.91 638.5 Embodiment 23 yes 230.4 1.94 580.7 Embodiment 24 yes 230.4 1.94 580.7 Comparative Example 1 no 183.5 1.81 640.4 Comparative Example 2 no 192.8 1.72 680.4 Comparative Example 3 no 185.2 1.82 666.2 Comparative Example 4 yes 140.3 1.55 565.0 Comparative Example 5 yes 220.9 1.54 535.0 Analyzing Example 1 in conjunction with the accompanying drawings, the DSC curve of the molten salt of this component has only one melting peak within the test range, and no secondary peak appears, which is a eutectic salt with a melting point of 182.3 °C. Figure 1 As shown in Figure 2, the average specific heat capacity between 200 and 500 °C is 1.81 J / g∙K, which is consistent with the predicted value. Figure 2 As shown; the extrapolated decomposition temperature is 678.5 ℃, as Figure 3 shown.
[0057] Combined with the accompanying drawings, the comparative example 1 is analyzed. The DSC curve of the molten salt of this component shows two melting peaks within the test range, and the secondary peak is more obvious, such as Figure 4 The part surrounded by the red dotted line is a non-eutectic salt, and its melting point when completely melted is 183.5 °C.
[0058] As can be seen from Table 2, the minimum eutectic point temperature of the multi-element eutectic molten salt of the present invention is 180.0 °C, the maximum thermal decomposition temperature can reach 678.5 °C, and the average specific heat capacity of the liquid segment within the test range is greater than (equal to) 1.81 J / g∙K. It has a low melting point, high stability, and high specific heat capacity, and can be used as a heat transfer and storage medium in solar thermal power generation, compressed air energy storage, industrial waste heat recovery, molten salt heat pump heat storage, off-peak electricity thermal storage heating, and flexibility transformation of thermal power plants.
[0059] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.
Claims
1. A high-stability multi-element eutectic molten salt, characterized in that: The high-stability multi-component eutectic molten salt is composed of single-component salts in the following weight percentages: 32.0~56.0wt.% NaNO3, 40.0~60.0wt.% NaNO2, 0~10.0%wt.Na2CO3, and 0~13.0wt.% KNO2.
2. The high-stability multi-element eutectic molten salt according to claim 1, characterized in that: The high-stability multi-component eutectic molten salt is composed of single-component salts with the following weight percentages: 40.0-56.0 wt.% NaNO3, 44.0-60.0 wt.% NaNO2.
3. The high-stability multi-element eutectic molten salt according to claim 1, characterized in that: The high-stability multi-component eutectic molten salt is composed of single-component salts with the following weight percentages: 35.0-55.0 wt.% NaNO3, 43.0-58.0 wt.% NaNO2, and 1.0-10.0 wt.% Na2CO3.
4. The high-stability multi-element eutectic molten salt according to claim 1, characterized in that: The high-stability multi-component eutectic molten salt is composed of single-component salts in the following weight percentages: 35.0-52.0wt.% NaNO3, 40.0-55.0wt.% NaNO2, and 1.0-13.0wt.% KNO2.
5. The high-stability multi-element eutectic molten salt according to claim 1, characterized in that: The high-stability multi-component eutectic molten salt is composed of single-component salts in the following weight percentages: 32.0-52.0wt.% NaNO3, 42.0-60.0wt.% NaNO2, 1.0-10.0wt.% Na2CO3, and 1.0-13.0wt.% KNO2.
6. A method for preparing a high-stability multi-element eutectic molten salt according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, drying the single-component salt raw materials separately; S2. Weigh the single-component salt in the formula, grind, and mix evenly to obtain a mixed salt; S3, placing the mixed salt in a muffle furnace to melt to obtain a molten salt, cooling the molten salt to room temperature, and grinding to obtain a high-stability multi-element eutectic molten salt; The temperature rise procedure of the muffle furnace is as follows: from room temperature to 100-120 °C, constant temperature for 12-24 h, and a heating rate of 5-10 K / min; from 100-120 °C to 300-450 °C, constant temperature for 12-24 h, and a heating rate of 5-10 K / min.
7. The high-stability multi-element eutectic molten salt described in any one of claims 1-5 is used as a heat transfer / heat storage medium in the fields of solar thermal power generation, compressed air energy storage, industrial waste heat recovery, molten salt heat pump heat storage, off-peak electric thermal storage heating, and flexibility transformation of thermal power plants.
Citation Information
Patent Citations
Method for improving nitrite salt compositions used as heat transfer medium or heat storage medium
CN104583357A