Preparation method of special anti-corrosion and anti-rust agent for brake fluid
Through the combination of silicone oil-modified polyurethane epoxy resin and solid boric acid anti-rust agent, the problem of insufficient adhesion ability of anti-corrosion anti-rust agent for brake fluid is solved, the anti-corrosion performance and adhesion are improved, the service life is extended, and the reason for the prevention and treatment of the anti-corrosion agent is avoided. The temperature-induced curing ensures the fluidity and corrosion resistance of the brake fluid.
Patent Information
- Application Number
- CN202410971032.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing anti-corrosion and rust agents for brake fluid have weak adhesion capabilities and are prone to falling off. They cannot effectively prevent corrosion of metal parts, resulting in rust and affecting service life.
The combination of silicone oil-modified polyurethane epoxy resin and solid boric acid anti-rust agent is used to improve the adhesion of anti-corrosion anti-rust agent through specific mixing and drying treatment steps, and the adhesion between boric acid and metal is used to suppress water and metal. Contact, store in combination with specific temperatures to extend service life.
It significantly improves the adhesion and corrosion resistance of anti-corrosion agents, extends the service life, avoids curing caused by excessive temperature of brake fluid, improves viscosity and flowability, and prevents corrosion of metal and rubber parts.
Smart Images

Figure CN118931622A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-corrosion and anti-rust agents, and in particular to a method for preparing an anti-corrosion and anti-rust agent special for brake fluid. Background Art
[0002] Brake fluid is a liquid medium that transmits brake pressure in a hydraulic brake system and is used in vehicles with a hydraulic brake system. Brake fluid, also known as brake oil or force oil, is an indispensable part of the brake system. In the brake system, it serves as a force transmission medium. Because liquid cannot be compressed, the pressure output from the master cylinder will be directly transmitted to the slave cylinder through the brake fluid. During the use of brake fluid, an anti-corrosion and rust inhibitor is required to be used in conjunction with it. However, the existing anti-corrosion and rust inhibitor for brake fluid has weak adhesion and is prone to coating shedding. When used with brake fluid, it will not be able to prevent corrosion and rust on metal parts, and sometimes causes metal parts to be corroded, resulting in a large amount of rust on their surface, affecting their service life. Summary of the invention
[0003] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0004] A method for preparing a special anticorrosion and rust inhibitor for brake fluid comprises the following steps:
[0005] Step 1: Selection of experimental tools;
[0006] Step 2: Material selection and weighing;
[0007] Step 3: Mix and stir;
[0008] Step 4: Drying;
[0009] Step 5: Mix and stir for the second time;
[0010] Step 6: Store at specific temperature.
[0011] A further improvement of the technical solution of the present invention is that: in the step one, multiple volumetric flasks, magnetic stirrers, electronic balances, multiple beakers and laboratory ovens need to be prepared in advance, and after the experimental equipment is selected, each experimental equipment needs to be disinfected with alcohol disinfectant to avoid affecting the purity of the subsequent preparation of the preservative and rust inhibitor.
[0012] A further improvement of the technical solution of the present invention is that: in the step 2, boric acid, water, acetic acid, sodium hydroxide, hydroxyl silicone oil, diisocyanate, a catalyst and glycidol need to be selected, and an electronic balance needs to be used to weigh 10 grams of boric acid, 2 grams of sodium hydroxide, and 3 grams of glycidol respectively, and 70 milliliters of water, 5 milliliters of acetic acid, 10 milliliters of diisocyanate and 3 milliliters of catalyst are measured respectively using multiple prepared volumetric flasks.
[0013] A further improvement of the technical solution of the present invention is that: an empty volumetric flask is selected, 10 grams of boric acid in step 2 is added to the volumetric flask, and 50 milliliters of water is poured into it, and finally it is stirred by using a prepared magnetic stirrer until the boric acid in the volumetric flask is completely dissolved, and the stirring is stopped to obtain solution A.
[0014] A further improvement of the technical solution of the present invention is that: the prepared 5 ml of acetic acid is added to the A solution, and then 2 g of sodium hydroxide is added, and a magnetic stirrer is used to stir the solution until the solution is stirred into a white mixture, thereby obtaining the B solution.
[0015] A further improvement of the technical solution of the present invention is that: the B solution is poured into the beaker prepared in step 1, and then the beaker is placed in a laboratory oven and dried until it is completely solidified, thereby obtaining a solid boric acid rust inhibitor, and finally it is taken out and placed at room temperature for 10-15 minutes, and after it is cooled, it is stored in a dark place for subsequent use.
[0016] A further improvement of the technical solution of the present invention is that: the step three also includes selecting an empty volumetric flask, pouring 10 ml of weighed diisocyanate into it, and vacuum dehydrating it at 90-120 degrees Celsius until it is completely dehydrated, leaving it to stand until its temperature drops to 60-80 degrees Celsius, then adding 10 ml of diisocyanate and 3 ml of catalyst, reacting at a temperature of 60-80 degrees Celsius, the reaction process is 1-5 hours, and finally adding 3 grams of propylene oxide, at this time, the temperature needs to be controlled between 40-70 degrees Celsius, and reacting for 1-3 hours, thereby obtaining a silicone oil-modified polyurethane epoxy resin.
[0017] A further improvement of the technical solution of the present invention is that the prepared silicone oil modified polyurethane epoxy resin and solid boric acid rust inhibitor are poured into an empty volumetric flask, 20 ml of water is added, and the mixture is stirred by a magnetic stirrer until the silicone oil modified polyurethane epoxy resin and the solid boric acid rust inhibitor are completely dissolved in the water, thereby obtaining a special anticorrosion and rust inhibitor for brake fluid.
[0018] A further improvement of the technical solution of the present invention is that the anticorrosion and rust inhibitor obtained in step five is poured into a beaker and stored in an environment with a temperature of 30-50 degrees Celsius to prevent it from solidifying.
[0019] Due to the adoption of the above technical solution, the present invention has the following technical advances compared with the prior art:
[0020] 1. The present invention provides a method for preparing a special anticorrosion and rust inhibitor for brake fluid. The overall adhesion of the anticorrosion and rust inhibitor can be improved through the joint action of silicone oil-modified polyurethane epoxy resin and solid boric acid rust inhibitor. Because the solid boric acid rust inhibitor contains boric acid and sodium hydroxide, the good adhesion between boric acid and metal can be utilized, and the sodium hydroxide powder inhibits the contact between water and metal in the environment, which can further improve the anticorrosion performance and adhesion of the anticorrosive coating. Finally, the anticorrosion and rust inhibitor is stored at a specific temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a structural schematic diagram of the preparation method of the special anticorrosion and rust inhibitor for brake fluid of the present invention. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below in conjunction with embodiments:
[0023] Example 1
[0024] like Figure 1 As shown, the present invention provides a method for preparing a special anticorrosion and rust inhibitor for brake fluid, comprising the following steps:
[0025] Step 1: Selection of experimental tools;
[0026] Step 2: Material selection and weighing;
[0027] Step 3: Mix and stir;
[0028] Step 4: Drying;
[0029] Step 5: Mix and stir for the second time;
[0030] Step 6: Store at specific temperature.
[0031] Example 2
[0032] like Figure 1 As shown, on the basis of Example 1, the present invention provides a technical solution: preferably, in the step 1, a plurality of volumetric flasks, a magnetic stirrer, an electronic balance, a plurality of beakers and a laboratory oven need to be prepared in advance, and after the experimental equipment is selected, each experimental equipment needs to be disinfected with an alcohol disinfectant to avoid affecting the purity of the subsequent preparation of the anticorrosion and rust inhibitor;
[0033] In the step 2, boric acid, water, acetic acid, sodium hydroxide, hydroxyl silicone oil, diisocyanate, catalyst and glycidol need to be selected. Here, an electronic balance needs to be used to weigh 10 grams of boric acid, 2 grams of sodium hydroxide and 3 grams of glycidol respectively. 70 milliliters of water, 5 milliliters of acetic acid, 10 milliliters of diisocyanate and 3 milliliters of catalyst are respectively measured with multiple prepared volumetric flasks. An empty volumetric flask is selected, 10 grams of boric acid in step 2 is added to the volumetric flask, and 50 milliliters of water is poured into it. Finally, it is stirred by using the prepared magnetic stirrer until the volume in the volumetric flask is 100 grams. When the boric acid is completely dissolved, stirring is stopped to obtain solution A, wherein 5 ml of the prepared acetic acid is added to solution A, and then 2 g of sodium hydroxide is added, and a magnetic stirrer is used to stir the solution until the solution is stirred into a white mixture, thereby obtaining solution B, wherein solution B is poured into the beaker prepared in step 1, and then the beaker is placed in a laboratory oven and dried until completely solidified, thereby obtaining a solid boric acid rust inhibitor, and finally taken out and placed at room temperature for 10-15 minutes, and after cooling, stored in a dark place for subsequent use;
[0034] The step three also includes selecting an empty volumetric flask, pouring 10 ml of the weighed diisocyanate into it, and vacuum dehydrating it at 90-120 degrees Celsius until it is completely dehydrated, leaving it to stand until its temperature drops to 60-80 degrees Celsius, then adding 10 ml of diisocyanate and 3 ml of catalyst, reacting at a temperature of 60-80 degrees Celsius, and the reaction process is 1-5 hours, and finally adding 3 grams of glycidol, at this time, the temperature needs to be controlled between 40-70 degrees Celsius, and reacting for 1-3 hours, thereby obtaining a silicone oil-modified polyurethane epoxy resin, the prepared silicone oil-modified polyurethane epoxy resin and solid boric acid rust inhibitor are poured into an empty volumetric flask, and 20 ml of water are added, and the mixture is stirred by a magnetic stirrer until the silicone oil-modified polyurethane epoxy resin and the solid boric acid rust inhibitor are completely dissolved in water, thereby obtaining a special anticorrosion and rust inhibitor for brake fluid;
[0035] The anticorrosion and rust inhibitor obtained in step five is poured into a beaker and stored in an environment with a temperature of 30-50 degrees Celsius to prevent it from solidifying.
[0036] In this embodiment, the overall adhesion of the anti-corrosion and rust inhibitor can be improved through the combined action of silicone oil-modified polyurethane epoxy resin and solid boric acid rust inhibitor. Because the solid boric acid rust inhibitor contains boric acid and sodium hydroxide, the good adhesion between boric acid and metal can be utilized, and the sodium hydroxide powder inhibits the contact between water and metal in the environment, which can further improve the anti-corrosion performance and adhesion of the anti-corrosion coating. Finally, in the storage of the anti-corrosion and rust inhibitor, it is placed at a specific temperature for storage, which can extend its service life and prevent it from solidifying due to excessively high temperature. It can extend its service life and prevent it from solidifying due to excessively high temperature. It can improve the viscosity-temperature property of the brake fluid and improve its fluidity. It will not cause corrosion or deterioration of metal and rubber parts during use.
[0037] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.
Claims
1. A method for preparing a special anticorrosion and rust inhibitor for brake fluid, The method comprises the following steps: Step 1: Selection of experimental tools; Step 2: Material selection and weighing; Step 3: Mix and stir; Step 4: Drying; Step 5: Mix and stir for the second time; Step 6: Store at specific temperature.
2. The method for preparing a special anticorrosion and rust inhibitor for brake fluid according to claim 1, characterized in that: In the step 1, multiple volumetric flasks, magnetic stirrers, electronic balances, multiple beakers and laboratory ovens need to be prepared in advance. After the experimental equipment is selected, each experimental equipment needs to be disinfected with alcohol disinfectant to avoid affecting the purity of the subsequent preparation of the preservative and rust inhibitor.
3. The method for preparing a special anticorrosion and rust inhibitor for brake fluid according to claim 1, characterized in that: In the step 2, boric acid, water, acetic acid, sodium hydroxide, hydroxyl silicone oil, diisocyanate, catalyst and glycidol need to be selected. Here, an electronic balance needs to be used to weigh 10 grams of boric acid, 2 grams of sodium hydroxide, and 3 grams of glycidol respectively, and 70 milliliters of water, 5 milliliters of acetic acid, 10 milliliters of diisocyanate and 3 milliliters of catalyst are measured respectively using multiple prepared volumetric flasks.
4. The method for preparing a special anticorrosion and rust inhibitor for brake fluid according to claim 1, characterized in that: Select an empty volumetric flask, add 10 grams of boric acid in step 2 into the volumetric flask, pour 50 milliliters of water into it, and finally stir it with a prepared magnetic stirrer until the boric acid in the volumetric flask is completely dissolved, then stop stirring to obtain solution A.
5. The method for preparing a special anticorrosion and rust inhibitor for brake fluid according to claim 4, characterized in that: The prepared 5 ml of acetic acid is added to solution A, and then 2 g of sodium hydroxide is added, and a magnetic stirrer is used to stir the solution until the solution is stirred into a white mixture, thereby obtaining solution B.
6. The method for preparing a special anticorrosion and rust inhibitor for brake fluid according to claim 5, characterized in that: The B solution is poured into the beaker prepared in step 1, and then the beaker is placed in a laboratory oven and dried until completely solidified to obtain a solid boric acid rust inhibitor. Finally, it is taken out and placed at room temperature for 10-15 minutes. After it cools, it is stored in a dark place for subsequent use.
7. The method for preparing a special anticorrosion and rust inhibitor for brake fluid according to claim 3, characterized in that: The step three also includes selecting an empty volumetric flask, pouring 10 ml of weighed diisocyanate into it, and vacuum dehydrating it at 90-120 degrees Celsius until it is completely dehydrated, leaving it to stand until its temperature drops to 60-80 degrees Celsius, then adding 10 ml of diisocyanate and 3 ml of catalyst, reacting at a temperature of 60-80 degrees Celsius, the reaction process is 1-5 hours, and finally adding 3 grams of propylene oxide, at this time, the temperature needs to be controlled between 40-70 degrees Celsius, and reacting for 1-3 hours, thereby obtaining a silicone oil-modified polyurethane epoxy resin.
8. The method for preparing a special anticorrosion and rust inhibitor for brake fluid according to claim 7, characterized in that: The prepared silicone oil modified polyurethane epoxy resin and solid boric acid rust inhibitor are poured into an empty volumetric flask, and 20 ml of water is added, and the mixture is stirred by a magnetic stirrer until the silicone oil modified polyurethane epoxy resin and the solid boric acid rust inhibitor are completely dissolved in the water, thereby obtaining a special anticorrosion and rust inhibitor for brake fluid.
9. The method for preparing a special anticorrosion and rust inhibitor for brake fluid according to claim 8, characterized in that: The anticorrosion and rust inhibitor obtained in step five is poured into a beaker and stored in an environment with a temperature of 30-50 degrees Celsius to prevent it from solidifying.