Method for improving segregation of solute sulfur in sulfur-containing special steel casting blank
By introducing tellurium elements during steel smelting to form MnS-MnTe composite inclusions, the problem of sulfur segregation in special sulfur-containing steel billets is solved, and the mechanical and corrosion resistance of the material is significantly improved, and the casting quality is improved.
Patent Information
- Application Number
- CN202411017340.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
Sulfur segregation problems often exist in special sulfur-containing steel castings, resulting in uneven material properties, affecting its mechanical properties, corrosion resistance and casting quality.
In the process of steel smelting, an appropriate amount of tellurium element is introduced, and by feeding tellurium core wire, MnS-MnTe composite inclusions are formed, which improves the sulfide morphology and distribution and reduces the segregation of sulfur.
It effectively reduces the segregation index of sulfur, improves the high-temperature strength, plastic toughness and cutting performance of the casting billet, and makes the material performance more uniform and stable.
Smart Images

Figure CN118932138A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a method for improving the segregation of solute sulfur in sulfur-containing special steel ingots. Background Art
[0002] Sulfur-containing special steel is an energy-efficient steel grade developed along with the international energy shortage. It has special structures and properties that meet specific industrial needs. Sulfur usually exists as a non-metallic element in special steel, affecting the mechanical properties and processing properties of steel. According to the sulfur content, special steel can be divided into quenched and tempered steel (S≤0.025%), non-quenched and tempered steel (S=0.025%~0.065%), gear steel (S=0.025~0.035%) and free-cutting steel (S=0.08~0.30%). With the addition of S element, it has a negative impact on the ingot and surface quality of sulfur-containing special steel, and it is easy to have surface cracks on the ingot and sulfur segregation in the ingot. With the transformation and upgrading of downstream industries, users have higher and higher requirements for the quality of steel, and how to improve the defects of ingots is very important.
[0003] Segregation is a common defect in the casting process of metal materials, which will lead to uneven material properties. Sulfur segregation is mainly formed during metal smelting and casting due to the uneven redistribution of solute elements between solid and liquid phases. During the solidification process, due to the growth of columnar crystals, the solute elements in the unsolidified molten steel between dendrites are enriched. At the same time, due to the bulging of the billet and the solidification shrinkage at the end of the liquid phase hole, a central suction force is generated, causing the solute elements to gather in the central area, thereby forming sulfur segregation. In addition, when the columnar crystals of the continuous casting billet are well developed, especially when the columnar crystals are overdeveloped, the continuous casting billet is prone to "bridging" phenomenon, making the central segregation more serious.
[0004] Segregation will make the internal composition of the grains in the material uneven, resulting in reduced mechanical properties, especially plasticity and toughness. This is a serious defect for load-bearing castings and may cause failure during use. In addition, the uneven composition caused by segregation will reduce the corrosion resistance of the material. In some applications that require high corrosion resistance, the presence of segregation will greatly affect the service life of the material. Both grain boundary segregation and regional segregation will increase the tendency of the material to thermal crack. In high-temperature applications, this defect may cause cracking of the material, thereby reducing its reliability. The material inhomogeneity caused by segregation is also one of the root causes of fatigue cracks, which will significantly reduce the fatigue life of the material. Segregation may also affect the casting molding properties of the material, such as the uneven surface of the casting or internal voids.
[0005] In order to reduce the harm of segregation, a series of measures are usually needed, such as controlling the cooling rate of the casting process, using appropriate alloy elements, and performing subsequent heat treatment, etc. Through these methods, segregation can be controlled or eliminated to a certain extent, thereby improving the quality and performance of metal materials.
[0006] CN202310950344.8 discloses a method for reducing the casting segregation of sulfur-based free-cutting steel in small square billets, and the method obtains sulfur-based free-cutting steel in small square billets with reduced casting segregation through crystallizer cooling, crystallizer electromagnetic stirring, secondary cooling chamber cooling, and terminal electromagnetic stirring. 202310352628.7 discloses a production method for improving the segregation of continuous casting billets of sulfur-containing steel grades, and the method detects the high-temperature thermoplasticity curve and adjusts the light pressure during the continuous casting process according to the S content to improve the segregation of the billet. The above methods have a certain effect on controlling the segregation of the billet, but the method of adjusting the terminal electromagnetic stirring and light pressure is more complicated.
[0007] Tellurium is located between selenium and polonium in the sixth main group of the periodic table, with a melting point of 452°C and a boiling point of 1390°C. Tellurium coexists with sulfides in steel, which can optimize the morphology of sulfides, improve their grade, reduce magnetic trace defects, and improve the cutting performance of materials. Tellurium can regulate the type of sulfides, transforming rod-shaped sulfides into ellipsoidal sulfides, preventing sulfides from deforming into long strips along the rolling direction, improving the grade of sulfides, and at the same time improving the segregation of sulfur elements. Summary of the invention
[0008] The purpose of the present invention is to provide a method for improving the solute sulfur segregation in sulfur-containing special steel ingots, so as to overcome the sulfur segregation problem commonly existing in sulfur-containing special steels, improve the performance of the product, and make the sulfur-containing steel have good high-temperature strength, plasticity and toughness and cutting performance.
[0009] To achieve the above object, the technical solution of the present invention is:
[0010] A method for improving the segregation of solute sulfur in sulfur-containing special steel ingots, the process flow is converter smelting → LF furnace refining → VD / RH furnace refining → feeding tellurium cored wire → continuous casting, characterized in that: in the chemical composition of the steel, C=0.05-0.90%, Si=0.05-0.75%, Mn=0.50-1.50%, P≤0.045%, S=0.0015%-0.40%, Te=0.0005%-0.03%, and Te / S=0.01-1.0; the steps of feeding Te cored wire are as follows: when RH At the end of refining, after sampling and testing the composition to meet the requirements, tellurium-containing cored wire is fed in, the wire feeding speed is 80-150m / min, and the elemental composition of the cored wire is Fe=70%-80%, Te=10%-20%, S=5%-15%; after the wire feeding is completed, the surface of the molten steel needs to be covered with carbonized rice husks; after reducing the argon flow rate to around 10L / min, continue soft blowing for 5-20min; when the temperature is 1585-1595℃, the bag is hoisted on the turntable; in order to increase the tellurium wire recovery rate, the wire feeding tube should be vertically inserted into the molten steel, and the outlet of the wire feeding machine should be less than 20cm away from the molten steel surface.
[0011] Preferably, when the sulfur-containing special steel is non-quenched and tempered steel, in the chemical composition mass percentage of the steel, S=0.035%, Te=0.0030%, Te / S=0.086, the continuous casting billet size is 240 mm square billet; and the sulfur segregation index is 0.93-1.14.
[0012] Preferably, when the sulfur-containing special steel is free-cutting steel, the chemical composition of the steel has a mass percentage of S=0.37%, Te=0.010%, and Te / S=0.027, the continuous casting billet size is 150 mm square billet; and the sulfur segregation index is 0.96-1.05.
[0013] Preferably, when the sulfur-containing special steel is gear steel, the chemical composition of the steel has a mass percentage of S=0.020%, Te=0.0060%, and Te / S=0.03, the continuous casting billet size is 340 mm square billet; and the sulfur segregation index is 0.95-1.02.
[0014] Principle of the invention:
[0015] (1) Tellurium and sulfur are elements of the same main group, with similar physical and chemical properties; sulfur and tellurium cannot form compounds, but they are mutually soluble in the molten state; tellurium is almost insoluble in the steel matrix at room temperature, and usually tellurium is associated with sulfur; when a trace amount of tellurium is added to steel, tellurium can usually be dissolved in manganese sulfide to form a (Mn,Te)S solid solution. When the tellurium content is high, a composite inclusion of Mn(S,Te)-MnTe can be formed;
[0016] (2) Since tellurium acts as a surfactant and preferentially accumulates at interfaces, one is at the inclusion-metal interface; the other is at the solid-liquid interface during the solidification of molten steel. In addition, due to the thermodynamic similarity between Te and S, tellurium solute is redistributed into the liquid phase and accumulates at the interface at the solidification front. Therefore, Te is believed to accumulate at the solid-liquid interface during the solidification of molten steel. The formation and advancement rate of the interface, which is affected by the solidification rate, also affects the diffusion direction of elements at the interface. When the solidification rate is low, before the next layer of solid phase is formed, the solute will have enough time to diffuse back to the liquid phase along the interface and tend to the equilibrium state because it is in a metastable state; when the solidification rate is faster, the solute diffusion time is shorter, and the excess solute relative to the equilibrium solubility will still be trapped in the solid phase.
[0017] Therefore, depending on the solidification rate, different degrees of local interface non-equilibrium may occur. (3) The S-Te interaction is weaker than the Fe-S interaction, while the formation of MnTe compounds infers that the Mn-Te interaction is stronger than the Fe-Mn interaction. Te, as a surfactant, can not only reduce the activation energy between the oxide and the steel liquid, but also inhibit the precipitation of MnS inclusions in the interdendritic region, indicating that Te affects the segregation of Mn and S. The presence of tellurium affects the reverse diffusion rate of solutes from the solid phase to the liquid phase during solidification. This diffusion rate will pass through the advancing solid-liquid interface and reduce the segregation of S. This is also one of the mechanisms by which Te changes the morphology of MnS inclusions; in addition, tellurium adsorption on the MnS surface slows down the deposition rate of growth units, thereby reducing the growth rate of inclusions.
[0018] The innovation of the present invention is to utilize the special function of tellurium to improve the macroscopic segregation effect of sulfur-containing steel, and to improve the solute sulfur segregation in the sulfur-containing special steel ingot by adding tellurium. Its technical effect is: by adding an appropriate amount of tellurium-containing cored wire in the steelmaking process to modify the MnS inclusions in the steel, the size of the MnS-MnTe composite inclusions formed after modification and regulation is increased and the distribution uniformity is improved, the precipitation of MnS inclusions in the interdendritic region is inhibited, the reverse diffusion rate of S is reduced, and the segregation of S is alleviated; at the same time, the MnS inclusions in the steel are modified into spherical inclusions, so that the distribution of inclusions in the steel is more uniform. The sulfur-containing special steel produced by the method of the present invention effectively improves the sulfur segregation in the continuous casting process, and the product performance is excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of sampling drill cuttings from ingot castings. DETAILED DESCRIPTION
[0020] Embodiment 1:
[0021] A method for improving the segregation of solute sulfur in sulfur-containing special steel ingots. The sulfur-containing steel provided in this embodiment is non-quenched and tempered steel, and the chemical composition of the steel is shown in Table 1. The production process is: converter smelting → LF furnace refining → feeding tellurium cored wire → continuous casting, and the continuous casting ingot size is 240 mm square ingot. The key process steps include:
[0022] 0.003% tellurium was added to the steel, and the tellurium-containing non-quenched and tempered steel in Example 1 was obtained through the above production process. In order to improve sulfur segregation, Te / S was controlled to 0.09. The sulfur segregation in the steel was measured by the nine-point method. The nine-point method for measuring sulfur segregation is as shown in the attached figure. Figure 1 The segregation results are shown in Table 2. After adding tellurium to the steel, the S segregation extreme is 0.009%, and the S segregation index is 0.93-1.14.
[0023] Embodiment 2:
[0024] A method for improving the segregation of solute sulfur in sulfur-containing special steel ingots. The sulfur-containing special steel provided in this embodiment is free-cutting steel, and the chemical composition of the steel is shown in Table 1. The production process is: converter smelting → LF furnace refining → VD / RH furnace refining (sulfur-containing free-cutting steel does not undergo this process) → feeding tellurium cored wire → continuous casting, and the continuous casting ingot size is 150 mm square ingot. The key process steps include:
[0025] 0.01% tellurium was added to the steel, and the tellurium-containing free-cutting steel in Example 2 was obtained through the above production process. In order to improve sulfur segregation, Te / S was controlled to 0.027. The S segregation in the steel was measured by the 9-point method, and the results are shown in Table 2. After adding tellurium to the steel, the extreme S segregation was 0.032%, and the S segregation index was 0.96-1.05.
[0026] Embodiment 3:
[0027] A method for improving the segregation of solute sulfur in a sulfur-containing special steel ingot. The sulfur-containing special steel in this embodiment is a tellurium-containing gear steel, and the chemical composition of the steel is shown in Table 1. The production process of the steel is: converter smelting → LF furnace refining → VD / RH furnace refining (sulfur-containing free-cutting steel does not undergo this process) → feeding tellurium cored wire → continuous casting, and the continuous casting ingot size is 340 mm square ingot. The key process steps include:
[0028] 0.006% tellurium was added to the steel, and the tellurium-containing gear steel in Example 3 was obtained through the above production process. In order to improve sulfur segregation, Te / S was controlled to 0.3. The sulfur segregation in the steel was measured by the 9-point method, and the results are shown in Table 2. After adding tellurium to the steel, the extreme difference of S segregation was 0.002%, and the S segregation index was 0.95-1.02.
[0029] Comparative Example 1:
[0030] The composition of the non-quenched and tempered steel in this comparative example is similar to that in Example 1, and the chemical composition of the steel is shown in Table 1. The production process is: converter smelting → LF furnace refining → continuous casting, and the continuous casting billet size is 240 mm square billet. The results of S segregation in the steel measured by the 9-point method are shown in Table 2, and the S segregation extreme is 0.003%, and the S segregation index is 0.92-1.17.
[0031] Comparative Example 2:
[0032] The free-cutting steel composition of this comparative example is similar to that of Example 1, and the chemical composition of the steel is shown in Table 1. The production process is: converter smelting → LF furnace refining → continuous casting, and the continuous casting billet size is 150 mm square billet. The S segregation results in the steel measured by the 9-point method are shown in Table 2, the S segregation extreme is 0.01%, and the S segregation index is 0.93-1.09.
[0033] Comparative Example 3:
[0034] The gear steel composition of this comparative example is similar to that of Example 1, and the chemical composition of the steel is shown in Table 1. The production process is: converter smelting → LF furnace refining → VD / RH furnace refining (sulfur-containing free-cutting steel does not undergo this process) → tellurium cored wire feeding → continuous casting, and the continuous casting billet size is 340 mm square billet. The results of S segregation in steel measured by the 9-point method are shown in Table 2, and the S segregation extreme is 0.0017%, and the S segregation index is 0.93-1.05.
[0035] Table 1 Specific composition of special steel in the embodiment (wt.%)
[0036]
[0037] Table 2 S content and segregation index at each position of the ingot in the embodiment
[0038]
Claims
1. A method for improving the segregation of solute sulfur in sulfur-containing special steel ingots, the process flow is converter smelting → LF furnace refining → VD / RH furnace refining → feeding tellurium cored wire → continuous casting, characterized in that: The chemical composition of the steel is as follows: C = 0.05-0.90%, Si = 0.05-0.75%, Mn = 0.50-1.50%, P ≤ 0.045%, S = 0.0015%-0.40%, Te = 0.0005%-0.03%, and Te / S = 0.01-1.0; the continuous casting billet size is 140-340 mm square billet, and the sulfur segregation index is 0.93-1.14; the steps of feeding Te cored wire are as follows: at the end of RH refining, the sampling and testing composition reaches the required After the wire feeding, the tellurium-containing cored wire is fed at a feeding speed of 80-150 m / min. The elemental composition of the cored wire is Fe=70%-80%, Te=10%-20%, and S=5%-15%. After the wire feeding is completed, the surface of the molten steel needs to be covered with carbonized rice husks. After reducing the argon flow rate to around 10 L / min, continue soft blowing for 5-20 minutes. When the temperature is at 1585-1595°C, the package is hoisted onto the turntable. In order to increase the tellurium wire recovery rate, the wire feeding tube should be vertically inserted into the molten steel, and the outlet of the wire feeding machine should be less than 20 cm away from the molten steel surface.
2. The method for improving the segregation of solute sulfur in sulfur-containing special steel ingot according to claim 1, characterized in that: The sulfur-containing special steel is a non-quenched and tempered steel. In terms of the chemical composition by mass percentage, S=0.035%, Te=0.0030%, Te / S=0.086, and the continuous casting billet size is a 240 mm square billet; the sulfur segregation index is 0.93-1.
14.
3. The method for improving solute sulfur segregation in sulfur-containing special steel ingot according to claim 1, characterized in that: When the sulfur-containing special steel is free-cutting steel, the chemical composition of the steel has a mass percentage of S=0.37%, Te=0.010%, and Te / S=0.027, the continuous casting billet size is 150mm square billet; and the sulfur segregation index is 0.96-1.
05.
4. The method for improving solute sulfur segregation in sulfur-containing special steel ingot according to claim 1, characterized in that: The sulfur-containing special steel is gear steel, and in the chemical composition mass percentage of the steel, S=0.020%, Te=0.0060%, and Te / S=0.03, the continuous casting billet size is 340mm square billet; the sulfur segregation index is 0.95-1.02.