Mo / Ni series waste catalyst recovery method

By combining sodium carbonate grinding and multiple water immersions with acid immersion and arc furnace curing, the problems of high energy consumption and pollution in the recycling of Mo/Ni-Al2O3-type waste catalysts are solved, and efficient recycling of molybdenum, nickel, aluminum and water are achieved. Resource saving simplifies the operation process.

CN118932179AInactive Publication Date: 2024-11-12湖北灵晓新材料科技有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411113777.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has problems such as high energy consumption, serious pollution, inability to completely separate metals, inconvenient operation and waste of water resources when recycling Mo/Ni-Al2O3-type waste catalysts, especially the dry and wet processes have their own defects.

Method used

Sodium carbonate and water grinding and roasting, through multiple water immersion and filtration, combined with acid immersion and arc furnace curing, the efficient recovery of molybdenum, nickel and aluminum is achieved, and water resources are recovered by multi-efficient evaporation, and energy is reduced through heat recovery. Consumption.

Benefits of technology

It achieves high recovery and high purity of molybdenum, nickel and aluminum, saves water resources and energy, simplifies operating procedures, reduces sewage generation, and improves recycling efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932179A_ABST
    Figure CN118932179A_ABST
Patent Text Reader

Abstract

The invention discloses a Mo / Ni series waste catalyst recovery method, and relates to the field of waste catalyst recovery. Comprising the following steps of molybdenum recovery and nickel and aluminum recovery, wherein nickel and aluminum are recovered from a filter cake (2) collected in the molybdenum recovery process. According to the method, molybdenum, nickel and aluminum can be recovered at the same time, the operation method is simple, the recovery rate is high, and finally, the average recovery rate of molybdenum can reach 95.8%, the purity exceeds 99.3%, the recovery rate of nickel is larger than 95.13%, and the recovery rate of aluminum exceeds 97%; meanwhile, recycled reclaimed water resources are efficiently utilized, generation of sewage is reduced, an efficient energy utilization mode is provided, and water resources and energy can be saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of waste catalyst recovery, and specifically to a method for recovering Mo / Ni-based waste catalysts, and in particular to a method for extracting useful metals from Mo / Ni-Al2O3-based waste catalysts. The method can effectively recover metals such as nickel, molybdenum, and aluminum in the catalysts. Background Art

[0002] my country is a country with large energy consumption. With the development of science and technology, catalysts play an important role in the efficient utilization of energy. According to statistics, more than 70% of industrial processes use catalysts, of which oil refining catalysts account for about 52% and chemical catalysts account for about 42%. Co and Mo catalysts with Al2O3 as carriers are the most common. As we all know, as the catalyst is used for a long time, some pollutants such as oil and coke accumulate on the active surface of the catalyst or block the pores of the catalyst, overheating causes the growth of active component particles and even sintering, the catalyst has poor crushing strength and causes particle breakage, and some poisons cause partial or complete loss of activity, which will cause the catalytic performance to decline. In order to ensure the stable and efficient operation of the system, the catalyst needs to be replaced. At present, the following methods are the most important for the treatment of Mo / Ni-Al2O3 waste catalysts in my country: (1) regeneration of the catalyst; (2) extraction of metal elements in the catalyst by certain methods; (3) landfill of waste catalysts.

[0003] In the early days, the treatment of Mo / Ni-Al2O3 waste catalysts usually adopted landfill and stacking, which not only occupied a large amount of land resources, but also the harmful substances in the waste catalysts would poison the land. At the same time, the waste Mo / Ni-Al2O3 catalysts would be washed by rainwater, and the toxic and harmful substances in them would spread around, polluting more land. More seriously, the toxic and harmful substances in them would be spread around by washing, causing water pollution, destroying the aquatic biological environment, and causing certain harm to the human body. Therefore, Mo / Ni-Al2O3 waste catalysts have been recorded in the national hazardous waste list as hazardous waste. At present, the most effective method for the treatment of Mo / Ni-Al2O3 waste catalysts is the extraction of metal elements.

[0004] The extraction of metal elements from Mo / Ni-Al2O3 waste catalysts can now be summarized into the following methods: (1) Dry recovery. This method is generally to calcine the waste catalyst together with a cosolvent and a reducing agent under high temperature conditions to react the metal components in the waste catalyst, and various non-ferrous metals are polymerized into alloys and filtered out together, while the carrier and the cosolvent form residues for removal. For example, Medvedev et al. reported that the molybdenum was recovered by calcining at a high temperature near the melting point of molybdenum and subliming the molybdenum at high temperature. Patent CN 100494423C uses Fe as a reducing agent to reduce and generate V-containing slag and Fe-Mo-Ni alloy, thereby realizing the recovery of V, Mo, and Ni. Patent CN110129573A oxidizes the molybdenum metal in the molybdenum-containing catalyst to form molybdenum oxide and sublimates the molybdenum oxide, thereby realizing the recovery of molybdenum in the catalyst. (2) Wet process, which uses acid, alkali or other solvents to achieve efficient leaching of valuable metals in the waste catalyst, and the leachate is then purified and impurized by ion exchange, extraction and other methods for recovery. Common wet process metallurgy can be divided into acid leaching and alkaline leaching. The two most commonly used acids in modern acid leaching processes are sulfuric acid and hydrochloric acid. Nitric acid, phosphoric acid and water-soluble organic acids such as citric acid and oxalic acid can also be used as leaching agents, while the most commonly used alkaline method is strong alkali or ammonia water. For example, Pinto et al. used sodium hydroxide solution to leach the waste catalyst with microwave assistance, and developed a simple, effective, low-cost and more environmentally friendly process to recover molybdenum from the alkaline leachate of the waste hydrodesulfurization catalyst; Patents CN113774219B, CN103769166 B, and CN111088438A all use acid leaching to extract cobalt and molybdenum. Patent CN 117660762 A mentions that the waste nickel-molybdenum catalyst after pretreatment is leached with sulfuric acid and hydrogen peroxide, and molybdenum is extracted with P227. After stripping with an alkaline reagent, high-purity molybdenum oxide is obtained; then Ni is extracted from the raffinate with a synergistic extractant containing Cyanex301 and TOP0, and then a high-purity nickel oxide product is obtained through hydrochloric acid stripping and precipitation with a precipitant. Patent CN100347318C dissolves the roasted and crushed waste cobalt and molybdenum catalyst powder with concentrated hydrochloric acid to prepare an acid-soluble clear liquid, thereby realizing the recovery of effective elements. Patent CN112342389A uses acid leaching followed by stripping to achieve efficient recovery of vanadium, molybdenum and nickel in waste catalysts; (3) Dry-wet combined process, the most common of which is the sodium roasting method. For example, L Shi et al. added CaO to the sodium salt and roasted it during the process of leaching molybdenum using sodium roasting. At this time, the molybdenum leaching rate was 97.5%. Patent CN115074554B uses oxygen-enriched roasting of waste catalysts, and then leaching the roasted products with acetic acid. After some reactions, molybdenum can be recovered. Patent CN112301227A uses oxidation roasting and leaching to recover metals such as vanadium, nickel, aluminum, and molybdenum.Patent CN113025834A uses sodium carbonate and waste catalysts to achieve molybdenum recovery after a series of reactions such as roasting and water immersion. Patent CN108067244B uses alkali and catalysts for roasting and then uses hot water immersion, filtration, ammonia analysis and other means to recover metals such as Mo and Ni. Patent CN112619658A extracts and removes oil from waste hydrogenation catalysts, roasts and removes carbon, crushes, and screens, then mixes with alkali, roasts, and soaks and filters the roasted waste catalyst powder with hot water to obtain filtrate and residue. After mixing and reacting with acid, the waste catalyst can be better recovered. Patent CN116751976A crushes, high-temperature roasts, ball mills, soaks, and removes impurities from the waste molybdenum catalyst raw materials in turn to obtain leached slag and purified liquid containing molybdenum and tungsten, and efficiently leaches and recovers molybdenum, tungsten, aluminum, nickel, etc. of the waste molybdenum catalyst, realizing the resource utilization of all components of the waste molybdenum catalyst. Patent CN103074494A adds alkali to the waste cobalt-molybdenum catalyst for roasting, then soaks it in water, washes it, filters it, and adds acid to adjust it, thereby realizing the recycling of the catalyst.

[0005] However, the general dry method needs to be carried out under high temperature conditions, with high reaction temperature, high energy consumption, serious pollution, and only alloy intermediate products can be obtained, and the metals cannot be completely separated. Although the acid leaching in the wet method has a high recovery rate, it is inconvenient to operate, produces a large amount of waste liquid, and has high requirements for equipment corrosion resistance. The NaOH method in the alkaline leaching method is generally combined with high-pressure leaching conditions, which has the advantages of easy control of conditions and fast leaching speed, but the leaching effect is not good for the preparation of catalysts with SiO2 as the carrier; the waste liquid pollution produced by the ammonia leaching method is relatively less toxic, but this method has high investment, long reaction time, and low leaching rate; the sodium method roasting operation is simple, widely used, and the principle is clear, but it requires high-temperature operating conditions, and the equipment is severely corroded during roasting. Leaching with water has low cost and low pollution, but there is an adsorption error of metal ions during leaching. Summary of the invention

[0006] The present invention provides a method for recovering Mo / Ni-based waste catalyst, aiming to solve the problems existing in the above-mentioned background technology.

[0007] In order to achieve the above technical objectives, the present invention mainly adopts the following technical solutions:

[0008] The present invention discloses a method for recovering Mo / Ni-based waste catalysts, comprising the following steps:

[0009] (1) Molybdenum recovery:

[0010] S11: grinding the waste catalyst, then adding sodium carbonate and water thereto, grinding again, standing and then roasting to obtain a roasted mixture;

[0011] S12: exchanging heat between the roasted mixture and desalted water to a set temperature, then soaking in water, and filtering the soaked material through a filter press to collect a primary filtrate and a filter cake (1), wherein the primary filtrate enters a primary filtrate collecting device, and the filter cake (1) enters a primary filter cake collecting device;

[0012] S13: mixing the collected filter cake (1) with desalted water, filtering with a filter press, collecting secondary filtrate and filter cake (2), wherein the secondary filtrate enters a secondary filtrate collecting device, and the filter cake (2) enters a secondary filter cake collecting device;

[0013] S14: adding an excess of calcium chloride to the primary filtrate, stirring, filtering through a filter press, collecting a tertiary filtrate and a filter cake (3), wherein the tertiary filtrate enters a tertiary filtrate collector, and the filter cake (3) enters a tertiary filter cake collecting device;

[0014] S15: acid leaching the filter cake (3), adjusting the pH to a suitable value, stirring, and filtering with a filter press to obtain an acid-containing filtrate and a filter cake (4); the filter cake (24) enters a molybdic acid collection tank to recover the molybdenum catalyst;

[0015] (2) Recovery of nickel and aluminum:

[0016] S21: drying the filter cake (2), adding coke thereto, mixing and grinding, and solidifying in an electric arc furnace to discharge nickel metal and aluminum oxide;

[0017] S22: Cooling the nickel metal element to room temperature through air cooling to form nickel element; purifying and drying the Al2O3 after cooling to obtain aluminum oxide.

[0018] In a preferred embodiment of the present invention, during the molybdenum recovery process, in the step S11, the amount of sodium carbonate added is 1.1-1.5 times the equivalent of the MoO3 content in the catalyst, and the amount of water added is 0.11-0.15 times the weight of the catalyst.

[0019] In a preferred embodiment of the present invention, during the molybdenum recovery process, in the step S11, after two grindings, both are sieved through a 160-300 mesh sieve, and after standing for 10-15 hours, a vacuum rotary kiln is used for roasting. The operating conditions of the vacuum rotary kiln are a pressure of -20--60Kpa, a temperature of 150-210°C, and a roasting time of 25-45min.

[0020] In a preferred embodiment of the present invention, during the molybdenum recovery process, in the step S12, the roasted mixture is heat exchanged with desalted water to 70-100°C, and then immersed in water with a secondary filtrate of 6-12 times the amount of the catalyst heated to 70-100°C. During the immersion in water, a stirrer with a rotation speed of 200-400rpm is used for continuous stirring, and the stirring time is 30-60min. The temperature is kept constant at 70-100°C during stirring. The material after immersion in water is filtered through a filter press after stirring for 40 minutes.

[0021] In a preferred embodiment of the present invention, during the molybdenum recovery process, in step S13, the collected filter cake (1) is mixed and stirred with 6-12 times the amount of desalted water as a catalyst, the stirring speed is set to 200-400 rpm, and the stirring time is 20-50 min.

[0022] In a preferred embodiment of the present invention, during the molybdenum recovery process, in step S14, the concentration of calcium chloride is 2.5-3.5 mol / L.

[0023] In a preferred embodiment of the present invention, during the molybdenum recovery process, in the step S14, the tertiary filtrate enters the tertiary filtrate collector and is treated by multi-effect evaporation, the generated water is reused, and the generated NaCl is purified and sold as a commodity.

[0024] In a preferred embodiment of the present invention, during the molybdenum recovery process, in step S15, the filter cake (3) is acid-leached with dilute hydrochloric acid, and then the pH is adjusted to 2-4, and the mixture is stirred sufficiently at a stirring speed of 200-400 rpm for 10-30 min.

[0025] In a preferred embodiment of the present invention, during the molybdenum recovery process, in step S15, after the acid-containing filtrate is concentrated, when the CaCl2 content in the acid-containing filtrate is greater than 2.5-3.5 mol / L, it is added to the primary filtrate.

[0026] In a preferred embodiment of the present invention, during the nickel and aluminum recovery process, in step S21, 1.0-2.5 Nm 3 / min hot air is used to dry the filter cake (2), and the filter cake is solidified at a temperature of 1600-1700°C, and nickel metal and 1.0-2.5Nm 3 / min air heat exchange cooling and then cooling to room temperature, and the heat generated during solidification is used to dry the filter cake (1), and the steam generated during drying is the heat source of desalted water and multiple-effect evaporator.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention can simultaneously recover molybdenum, nickel and aluminum from waste catalysts, has a simple operation method and a high recovery rate, and can ultimately achieve an average molybdenum recovery rate of 95.8%, a purity of more than 99.3%, a nickel recovery rate of more than 95.13%, and an aluminum recovery rate of more than 97%;

[0029] (2) The present invention makes efficient use of water resources in the recovery of waste catalysts, thereby reducing the generation of sewage, including: the secondary filtrate is used as the dissolving liquid during the first water immersion; secondly, the acid-containing filtrate is concentrated and added to the first filtrate to reduce the amount of water used when dissolving CaCl2; thirdly, the generated solution is concentrated by multi-effect evaporation, and the water is recycled, which is beneficial to saving water resources;

[0030] (3) The present invention provides a method for efficient use of energy in the recovery of waste catalysts, which is beneficial to energy conservation, including: 1. exchanging heat between the calcined mixture and desalted water to 70-100°C; 2. recovering the heat during solidification and cooling, and drying the filter cake (1), while generating a certain amount of steam as a heat source for desalted water and a multiple-effect evaporator. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A flow chart for sorting out the waste catalyst provided by the present invention;

[0032] Figure 2 A flow chart for recovering molybdenum from waste catalysts provided by the present invention;

[0033] Figure 3 This is a flow chart for recovering aluminum and nickel elements from waste catalysts provided by the present invention. DETAILED DESCRIPTION

[0034] After in-depth research, the applicant of the present invention has developed an efficient method for recovering waste catalysts. The method includes five sections: molybdenum element recovery, aluminum and nickel element recovery, heat recovery, sewage treatment and exhaust gas purification. It can achieve all-round and efficient recycling of waste catalysts, and ultimately achieve an average molybdenum recovery rate of 95.8%, a purity of more than 99.3%, a nickel recovery rate of more than 95.13%, and an aluminum recovery rate of more than 97%.

[0035] The specific process is as follows Figure 1As shown, a certain amount of waste catalyst is ground (200 meshes) and sampled (5 places). The content of MoO3 is analyzed by ICP (inductively coupled plasma spectrometer) and the average value is taken. The mass of sodium carbonate (1.2 times MoO3) and water (0.12 times catalyst) is calculated by the reaction mode (MoO3+Na2CO3=Na2MoO4+CO2). Sodium carbonate is weighed at 1.2 times the chemical equivalent, and water is weighed at 0.12 times the amount of waste catalyst. Then, the waste catalyst, sodium carbonate and water are mixed and ground again, sieved with 200 mesh and allowed to stand for 12 hours, and then roasted in a vacuum rotary kiln. The operating conditions of the vacuum rotary kiln are pressure -40Kpa and temperature 180°C. After roasting for 35 minutes, the roasted mixture is heat exchanged with desalted water to 90°C, and then soaked with secondary filtrate heated to 90°C with 9 times the amount of catalyst. During the soaking, a stirrer with a speed of 300rpm is used to stir continuously, and the stirring time is 40 minutes. The temperature is kept constant at 90°C during stirring. After stirring for 40 minutes, the soaked material is filtered through a filter press. The filtrate after filtration is called the primary filtrate. The primary filtrate is heat exchanged with the secondary filtrate and enters the primary filtrate collection device. The filter cake is called filter cake (1). The filter cake (1) is stored in a primary filter cake collection device. A 9-fold catalyst amount of desalted water is added to the collected filter cake (1) for secondary stirring. The second stirring speed is set at 300 rpm and the stirring time is 30 minutes. The second water immersion is performed. The material after the second water immersion is filtered again. The filtrate obtained after the filtration is entered into a secondary filtrate collection device. The filter cake (2) enters a secondary filter press filter cake (2) collection device.

[0036] Add 3.2 mol / L CaCl2 (CaCl2+Na2MoO4=CaMoO4+2NaCl, CaCl2+Na2CO3=CaCO3+2NaCl) of micro-superchemical equivalent to the primary filtrate, stir the reaction thoroughly, and the reacted material precipitates and enters the filter press, the tertiary filtrate enters the tertiary filtrate collector, and the filter cake (3) enters the filter cake (3) collector. The tertiary filtrate is treated by multi-effect evaporation, the water produced is reused, and the generated NaCl is purified and sold as a commodity. Add a certain amount of dilute hydrochloric acid to the filter cake (3), adjust the pH to 2-3, and then acid-leach the filter cake (3), stir thoroughly (stirring speed is 300 rpm, stirring time is 20 min) and react, and then filter press, the acid-containing filtrate enters the acid-containing filtrate collection tank, and the acid-containing filtrate is concentrated to a certain extent. When the CaCl2 content in the acid-containing filtrate is greater than 3.2 mol / L, it is added to the primary filtrate. The resulting filter cake is recorded as filter cake (4), and filter cake (4) enters the molybdic acid collection tank.

[0037] The effective elements contained in the secondary filter cake (2) include aluminum, nickel, etc. The filter cake (2) is dried using hot air, and a certain amount of coke is added to the dried filter cake (2) according to a certain chemical equivalent (2NiO+C=Ni+CO2), and the mixture is added to an electric arc furnace, and the filter cake is solidified at a temperature of 1650°C. The outflowing nickel metal element is cooled to room temperature by air cooling to form nickel element. The remaining Al2O3 is cooled, purified, dried and weighed.

[0038] In the description of the present invention, "room temperature" refers to 0-40°C, such as 10-30°C, 20-30°C, etc.

[0039] The present invention will be further described below in conjunction with specific examples. Specific examples are implemented under the premise of technical solutions of the present invention, and detailed implementation methods and operating procedures are provided. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for which specific conditions are not specified in the following examples are usually carried out under normal conditions. Unless otherwise indicated, ratios and percentages are by weight.

[0040] The instruments used in the following examples are shown in Table 1

[0041] Table 1 Reaction equipment

[0042]

[0043] An analytical balance (XY1000-1B) produced by Sartorius of Germany was used to weigh the required reagents, and the substances were analyzed using an inductively coupled plasma optical emission spectrometer (ICP-OES, Agilent 5800).

[0044] Example 1

[0045] 1.1 Recovery of Mo element

[0046] like Figure 2 As shown in the figure, the spent catalyst was ground, sieved (200 mesh) after grinding, mixed and sampled at different locations (5 locations) to analyze MoO3, NiO, Al2O using ICP (inductively coupled plasma spectrometer). 3 / The content of, see Table 2 for specific data,

[0047] Table 2 Main substance content

[0048]

[0049] Weigh 20g of waste catalyst, weigh 3.98g of sodium carbonate (industrial grade, 99.53%) after calculation, measure 2.4ml of desalted water, mix the waste catalyst (20g), sodium carbonate (3.98g), and water (2.4ml), and grind them. After grinding, let it stand for 12 hours to make the sodium carbonate disperse better in the waste catalyst. The mixture that has been standing is put into a vacuum rotary kiln for roasting. The pressure during roasting is controlled at -40Kpa, the temperature is 180℃, and the roasting is 35min. Roasting at this temperature has fewer side reactions. The calcined catalyst is heat exchanged with desalted water to recover its heat. When the temperature of the calcined material reaches 90°C, it is immersed in a constant temperature water immersion device together with 90°C, 180.00ml of secondary filtrate. Water immersion can better separate Mo from nickel and Al. Molybdenum exists in the form of Na2MoO4, and Al and Ni still exist in the form of their oxides. During immersion, a stirrer with a rotation speed of 300rpm is used for continuous stirring, and the constant temperature immersion time is 40min. The waste catalyst after water immersion is filtered. Under the action of the filter press, the filtrate containing Na2MoO4 and Na2CO3 is called the primary filtrate. The primary filtrate is heat exchanged with the secondary filtrate and enters the primary filtrate collection device when it is cooled to room temperature. The filter cake containing Al2O3 and CoO3 is called filter cake (1). The filter cake (1) is stored in a primary filter cake collection device. 180 ml of desalted water is added to the collected filter cake (1). The filter cake (1) is immersed in water for the second time. Stirring is continued during immersion. The second stirring speed is set at 300 rpm and the stirring time is 30 minutes. The material after the second immersion is filtered again. The filtrate obtained after the filtration enters the secondary filtrate collection device. The filter cake (2) enters the secondary filter cake (2) collection device. 13.0 ml of 3.2 mol / L CaCl2 (CaCl2+Na2MoO4=CaMoO4+2NaCl, CaCl2+Na2CO3=CaCO3+2NaCl) solution is added to the primary filtrate. After sufficient stirring and reaction, the reacted material is precipitated and enters the filter press. The tertiary filtrate enters the tertiary filtrate collector, and the filter cake (3) enters the filter cake (3) collector. The three filtrates were treated by multi-effect evaporation, the water produced was reused, and the generated NaCl was purified and sold as a commodity. The purified NaCl was weighed to be 4.4 g. The filter cake (3) in the collector was weighed after drying, and its mass was 4.23 g. Its purity was tested to be 99.25%. The recovery rate of molybdenum in the catalyst was calculated to be 94.1%.

[0050] 77.2 ml of 1.0 mol / L dilute hydrochloric acid was added to the filter cake (3) to fully stir the filter cake (3) (stirring speed was 300 rpm, stirring time was 20 min) for acid leaching. After sufficient reaction, the solution was adjusted to pH=2-3, and then pressure filtration was performed. The acid-containing filtrate entered the acid-containing filtrate collection tank. The acid-containing filtrate was concentrated to a certain extent. When the CaCl2 content in the acid-containing filtrate was greater than 3.2 mol / L, it was added to the primary filtrate. The resulting filter cake was recorded as filter cake (4), and the filter cake (4) entered the molybdic acid collection tank.

[0051] 1.2 Recovery of Co and Al elements

[0052] like Figure 3 As shown, the secondary filter cake (2) contains effective elements such as aluminum and nickel. 3 / min hot air is used to dry the filter cake (2). After drying, 0.5g of coke is added to the filter cake (2NiO+C=Ni+CO2), mixed and ground, and then added to an electric arc furnace. The filter cake is solidified at a temperature of 1650°C, and nickel metal and 1.5Nm 3 / min air heat exchange cooling and then cooling to room temperature, forming nickel single substance, the weight of which was weighed to be 0.78g. The remaining Al2O3 was cooled, purified and dried, and the weight of Al2O3 was weighed to be 13.89g.

[0053] Embodiment 2-6

[0054] The waste catalyst ground and analyzed in Example 1 was weighed 100g, 200g, 1000g, 2000g and 10kg respectively, and the recovery of Mo, Ni and Al elements was carried out according to the method of Example 1, wherein the mass of the waste catalyst in Example 2 was 100g, the mass of the waste catalyst in Example 3 was 200g, the mass of the waste catalyst in Example 4 was 1000g, the mass of the waste catalyst in Example 5 was 2000g, and the mass of the waste catalyst in Example 6 was 10kg. The amounts of other raw materials are detailed in Table 2, and the recovery amounts of Mo, Ni and Al elements are shown in Table 3.

[0055] Table 2 Raw material usage

[0056]

[0057]

[0058] Table 3 Mo, Ni, Al element recovery

[0059]

[0060] Example 7

[0061] Take a certain amount of 20g of waste catalyst, grind it (200 mesh), take samples (5 places), use ICP (inductively coupled plasma spectrometer) to analyze the content of MoO3, and take the average value. According to the reaction mode (MoO3+Na2CO3=Na2MoO4+CO2), 3.98g of sodium carbonate (industrial grade, 99.53%) is weighed after calculation; then the waste catalyst and sodium carbonate are ground again, and after standing, they are calcined in a rotary kiln. The operating conditions of the vacuum rotary kiln are pressure 20Kpa, temperature 700℃, and water immersion after calcination for 120min.

[0062] The remaining steps are carried out according to Example 1. Specific data are shown in Tables 4 and 5. Table 4 Raw material usage

[0063]

[0064]

[0065] Table 5 Mo, Ni, Al element recovery

[0066]

[0067] Comparing Example 1 with Example 7, it is found that the use of low-pressure and low-temperature roasting can effectively improve the recovery of Mo, Al, and Ni elements, and can also reduce the use of sodium carbonate, hydrochloric acid, and calcium chloride. The main reason is that under high temperature conditions, sodium carbonate and aluminum oxide undergo a side reaction (Na2CO3+Al2O3=2NaAlO2+CO2) to generate sodium metaaluminate, so that part of MoO3 fails to react completely. At the same time, NaAlO2 will undergo a certain hydrolysis reaction with CaCl2 after dissolving in water, and the use of dilute hydrochloric acid is increased during acid leaching. From the comparison of the examples, it is found that high-temperature roasting increases the use of raw materials and reduces the purity of the target product. Because part of MoO3 enters the filter cake (2), the purity of aluminum oxide after the reaction is reduced, the purity of metallic nickel is reduced, and the recovery rate is also reduced.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of the present invention. The above embodiment of the present invention can also be modified in various ways. That is, all simple, equivalent changes and modifications made according to the claims and the description of the present invention fall within the scope of protection of the claims of the present invention. The contents not described in detail in the present invention are all conventional technical contents.

Claims

1. A method for recovering Mo / Ni-based waste catalysts, characterized in that: The steps include: (1) Molybdenum recovery: S11: grinding the waste catalyst, then adding sodium carbonate and water thereto, grinding again, standing and then roasting to obtain a roasted mixture; S12: exchanging heat between the roasted mixture and desalted water to a set temperature, then soaking in water, and filtering the soaked material through a filter press to collect a primary filtrate and a filter cake (1), wherein the primary filtrate enters a primary filtrate collecting device, and the filter cake (1) enters a primary filter cake collecting device; S13: mixing the collected filter cake (1) with desalted water, filtering with a filter press, collecting secondary filtrate and filter cake (2), wherein the secondary filtrate enters a secondary filtrate collecting device, and the filter cake (2) enters a secondary filter cake collecting device; S14: adding an excess of calcium chloride to the primary filtrate, stirring, filtering through a filter press, collecting a tertiary filtrate and a filter cake (3), wherein the tertiary filtrate enters a tertiary filtrate collector, and the filter cake (3) enters a tertiary filter cake collecting device; S15: acid leaching the filter cake (3), adjusting the pH to a suitable value, stirring, and filtering with a filter press to obtain an acid-containing filtrate and a filter cake (4); the filter cake (24) enters a molybdic acid collection tank to recover the molybdenum catalyst; (2) Recovery of nickel and aluminum: S21: drying the filter cake (2), adding coke thereto, mixing and grinding, and solidifying in an electric arc furnace to discharge nickel metal and aluminum oxide; S22: Cooling the nickel metal element to room temperature through air cooling to form nickel element; purifying and drying the Al2O3 after cooling to obtain aluminum oxide.

2. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: During the molybdenum recovery process, in the step S11, the amount of sodium carbonate added is 1.1-1.5 times the equivalent of the MoO3 content in the catalyst, and the amount of water added is 0.11-0.15 times the weight of the catalyst.

3. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: During the molybdenum recovery process, in step S11, after two grindings, the molybdenum is sieved through a 160-300 mesh sieve, left to stand for 10-15 hours, and then roasted in a vacuum rotary kiln. The operating conditions of the vacuum rotary kiln are a pressure of -20--60Kpa, a temperature of 150-210°C, and a roasting time of 25-45min.

4. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: During the molybdenum recovery process, in step S12, the roasted mixture is heat exchanged with desalted water to 70-100°C, and then immersed in water with a secondary filtrate of 6-12 times the amount of the catalyst heated to 70-100°C. During the immersion, a stirrer with a rotation speed of 200-400rpm is used to stir continuously, and the stirring time is 30-60min. The temperature is kept constant at 70-100°C during stirring. The material after immersion in water is filtered through a filter press after stirring for 30-60 minutes.

5. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: During the molybdenum recovery process, in step S13, the collected filter cake (1) is mixed and stirred with 6-12 times the amount of desalted water as a catalyst, the stirring speed is set to 200-400 rpm, and the stirring time is 20-50 min.

6. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: During the molybdenum recovery process, in step S14, the concentration of calcium chloride is 2.5-3.5 mol / L.

7. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: During the molybdenum recovery process, in step S14, the tertiary filtrate enters the tertiary filtrate collector and is treated by multi-effect evaporation, the generated water is reused, and the generated NaCl is purified and sold as a commodity.

8. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: During the molybdenum recovery process, in step S15, the filter cake (3) is acid-leached with dilute hydrochloric acid, and then the pH is adjusted to 2-4, and the mixture is stirred sufficiently at a stirring speed of 200-400 rpm for a stirring time of 10-30 min.

9. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: During the molybdenum recovery process, in step S15, after the acid-containing filtrate is concentrated, when the CaCl2 content in the acid-containing filtrate is greater than 2.5-3.5 mol / L, it is added to the primary filtrate.

10. The method for recovering Mo / Ni-based waste catalyst according to claim 1, characterized in that: In the nickel and aluminum recovery process, in step S21, 1.0-2.5Nm 3 / min hot air is used to dry the filter cake (2), and the filter cake is solidified at a temperature of 1600-1700°C, and nickel metal and 1.0-2.5Nm 3 / min air heat exchange cooling and then cooling to room temperature, and the heat generated during solidification is used to dry the filter cake (1), and the steam generated during drying is the heat source of desalted water and multiple-effect evaporator.

Citation Information

Patent Citations

  • Wet separation technology for material containing lead, bismuth and molybdenum

    CN102321804A

  • Method for preparing high-purity nickel-based superalloy through integration of vacuum induction melting and electron beam refining

    CN112095030A

  • Method for recovering molybdenum in waste catalyst

    CN113025834A

  • Method for efficiently recovering valuable components in waste SCR (Selective Catalytic Reduction) catalyst

    CN115924926A

  • Method for recovering metals from waste aluminum catalyst

    US20140286840A1