Process for treating acidic gold-bearing minerals
By using isocyanuric acid halogenated derivatives as green-environmental gold-enriched agents, environmental pollution and safety hazards caused by the use of cyanide in the gold industry are solved, efficient leaching and environmentally friendly treatment of acidic gold-containing minerals are achieved, and process is simplified Process, suitable for different types of acidic gold-containing minerals.
Patent Information
- Application Number
- CN202410995086.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The traditional acid leaching process poses environmental pollution and safety risks in the gold industry, especially the difficulty in using cyanide and tailings treatment, and it is difficult to effectively treat acidic gold-containing minerals.
The halogenated derivatives of isocyanuric acid are used as green-environment-friendly gold-implanting agents. Through crushing treatment and pH adjustment, the gold leaching in acidic gold-containing minerals is achieved, which avoids the acid-base transformation process, simplifies the process flow, and is in an acidic environment. leaching is performed.
It realizes efficient leaching of gold, avoids the use of cyanide, simplifies the process flow, reduces the environmentally friendly treatment needs, and the pharmaceutical system is cyanobacterial and efficient, and is suitable for different types of acidic gold-containing minerals.
Smart Images

Figure CN118932186A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a process for treating acidic gold-containing minerals. Background Art
[0002] Cyanide gold leaching process is the mainstream gold extraction process in the gold industry. In recent years, in order to efficiently utilize difficult-to-treat gold-bearing ore resources, it is necessary to subject them to acid pretreatment, and the slag after the pretreatment process is acidic. In order to realize the subsequent cyanide gold leaching process of the acidic slag after the pretreatment process, it is necessary to introduce an acid-base transformation process into the leaching process, and then carry out the cyanide gold extraction process in an alkaline environment. However, cyanide is a highly toxic chemical, and its use, transportation, and storage are strictly restricted. At the same time, the tailings of cyanide gold leaching contain some cyanide and are classified as hazardous solid waste. Subsequently, relevant production enterprises are required to carry out strict environmental and safety treatment of the cyanide tailings. The traditional environmental protection treatment cycle is long, resulting in a large amount of cyanide tailings accumulation during the production process, which affects the smooth progress of the company's production.
[0003] In the traditional acid leaching process, such as the aqua regia method, the reaction is difficult to control during the gold leaching process, a large amount of toxic gas is generated, the tail gas treatment cost is high, and the equipment is seriously corroded. At present, a variety of non-cyanide gold leaching methods include thiosulfate method, glycine method, thiourea method, etc., while achieving cyanide-free gold leaching, it is impossible to avoid the introduction of acid-base transformation process. For example, the patent with publication number CN113462895A discloses an enhanced leaching method for complex and difficult-to-leach gold mines, which uses a catalytic oxidant AB-activator to pretreat the difficult-to-leach minerals, and then uses a super-brand environmentally friendly gold extraction agent to leach gold, wherein component A is a persulfate compound, component B is a peroxide compound, and the activator is a halogen compound ( The leaching system is composed of dichloroisocyanuric acid, trichloroisocyanuric acid, and chlorobromoisocyanuric acid. Sodium hydroxide is added to adjust the pH of the system to achieve the pretreatment of complex and difficult-to-leach gold ores. Due to the mutual restriction of the chemical properties of the catalytic oxidant AB-activator, the leaching system must be alkaline. The Chaofan brand environmentally friendly gold extraction agent is added under alkaline conditions to leach gold. The above process cannot avoid acid-base transformation and is difficult to effectively treat acidic minerals. At the same time, the main body of the reagent system and gold is the Chaofan brand environmentally friendly gold extraction agent, and the catalytic oxidant AB-activator is only a pretreatment agent. For the treatment of acidic gold-containing minerals, the limitations of traditional processes limit its market promotion.
[0004] In view of this, it is necessary to design an improved process for treating acidic gold-containing minerals to solve the above problems. Summary of the invention
[0005] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a process for treating acidic gold-containing minerals. By designing the components of the leaching agent system, the green and environmentally friendly extraction of gold from acidic gold-containing minerals can be achieved, so as to solve the environmental problems and safety hazards caused by the use of cyanide in the production process of gold enterprises and achieve green, environmentally friendly and sustainable development of the gold industry.
[0006] To achieve the above object, the present invention provides a process for treating acidic gold-bearing minerals, comprising the following steps:
[0007] S1. crushing the acidic gold-containing material, adding water to adjust the slurry to a mass percentage concentration of the slurry within a predetermined range;
[0008] S2. Add one or more of the green-environmentally friendly gold leaching agents to the slurry to make the green-environmentally friendly gold leaching agent reach a preset concentration; the green-environmentally friendly gold leaching agent is one or more halogenated derivatives of isocyanuric acid, and its general structural formula is In the formula, R 1 and R 2 Respectively represent one of Cl, Br and H;
[0009] S3. Add a pH adjuster to adjust the pH value of the slurry to a predetermined range, stir for a predetermined time at room temperature, and leach gold.
[0010] As a further improvement of the present invention, in step S1, the acidic gold-containing material includes one or more of biological oxidation slag, biological oxidation heap leaching slag, sulfuric acid slag, roasted sand and flotation gold concentrate.
[0011] As a further improvement of the present invention, the crushing process is to crush the material to a particle size of -0.074 mm, and the mineral powder accounts for 75% to 85% of the total mass of the material; the concentration of the ore slurry is 30% to 35%.
[0012] In the general structural formula of the green and environmentally friendly gold leaching agent, when R 1 When it is Cl, R 2 is Cl or H or Br; when R 1 When H, R 2 is Cl or Br; when R 1 When Br, R 2 It is Cl or H or Br.
[0013] As a further improvement of the present invention, in step S2, the concentration of the green-environmentally friendly gold leaching agent is 0.05-0.2 mol / L.
[0014] As a further improvement of the present invention, in step S3, the pH regulator is dilute hydrochloric acid, the predetermined range of the pH value of the slurry is 1 to 4, and the stirring time is 6 to 8 hours.
[0015] The beneficial effects of the present invention are:
[0016] 1. The present invention provides a process for treating acidic gold-containing minerals, using a halogenated derivative of isocyanuric acid to leach gold from acidic gold-containing minerals. The gold leaching agent not only achieves efficient leaching of gold from acidic materials, but also avoids the use of cyanide in the traditional gold industry from the source. In addition, the leaching system of the gold leaching agent is an acidic environment, which avoids the acid-base transition process, simplifies the process flow, and solves the acid-base transition difficulties of various acidic gold-containing minerals in the gold extraction process and the environmental problems caused by the traditional cyanide leaching process. The gold leaching agent used in the present invention is green and environmentally friendly, expanding the types of agents in the gold industry, and its potential application has broad prospects.
[0017] 2. In the gold leaching process of the present invention, the halogenated derivative of isocyanuric acid plays a dual role as an oxidant and a complexing agent. For example, when the halogenated derivative of isocyanuric acid is chloroisocyanuric acid, chloroisocyanuric acid can be mildly hydrolyzed to release high-valent chlorine (ClO - ), positive monovalent chloride (chloroisocyanuric acid, hypochlorite) and negative monovalent chloride ion (Cl - ) forms a redox potential pair, which maintains the potential stability of the system. In the process of chlorine reduction, gold can be oxidized, and the formed gold ions (III) can form extremely stable gold complexes with chloride ions. The consumption of chloride ions promotes the positive transformation of hypochlorite to chloride ions, and the consumption of hypochlorite further promotes the hydrolysis of chloroisocyanuric acid. In summary, through a series of reactions of halogenated derivatives of isocyanuric acid, the progressive chemical equilibrium is achieved, and finally the efficient leaching of gold is achieved. The entire process does not require acid-base transformation, and has excellent leaching effect under leaching conditions of normal temperature and pressure. The reagent system is cyanide-free, environmentally friendly, and efficient, and has poor corrosion to stainless steel leaching equipment, achieving the greatest balance between environmental protection and economy.
[0018] 3. The process for treating acidic gold-containing minerals of the present invention has a multi-layer gain effect compared with the traditional gold leaching process, solves the problem of acid-base transformation of acidic gold-containing materials, and the gold leaching agent in the process has good universality for minerals. From an environmental protection perspective, the leaching process does not require the introduction of subsequent environmental protection treatment procedures. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a flow chart of the preparation method of gold leaching agent A-7 in Example 8 of the present invention. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0021] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.
[0022] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0023] The present invention provides a process for treating acidic gold-bearing minerals, comprising the following steps:
[0024] S1. The acidic gold-containing material is crushed and water is added to adjust the slurry to a predetermined mass percentage concentration of the slurry.
[0025] Specifically, the acidic gold-containing material includes one or more of bio-oxidation slag, bio-oxidation heap leaching slag, sulfuric acid slag, roasted sand and flotation gold concentrate. The crushing treatment is to crush the material to a ore powder with an ore particle size of -0.074mm, which accounts for 75% to 85% of the total mass of the material, and the concentration of the slurry is preferably 30% to 35%.
[0026] S2. Add one or more green-environmentally friendly gold leaching agents to the slurry to make the green-environmentally friendly gold leaching agent reach a preset concentration; the green-environmentally friendly gold leaching agent is one or more halogenated derivatives of isocyanuric acid, and its general structural formula is In the formula, R 1 and R 2 They represent one of Cl, Br and H respectively.
[0027] Specifically, the concentration of the green and environmentally friendly gold leaching agent is 0.05 to 0.2 mol / L.
[0028] In the general structural formula of green and environmentally friendly gold leaching reagent, when R 1 When it is Cl, R 2 is Cl or H or Br; when R 1 When H, R 2 is Cl or Br; when R 1 When Br, R 2 It is Cl or H or Br.
[0029] S3. Add a pH adjuster to adjust the pH value of the slurry to a predetermined range, stir for a predetermined time at room temperature, and leach gold.
[0030] Specifically, the pH regulator is dilute hydrochloric acid, the predetermined range of the pH value of the slurry is 1 to 4, and the stirring time is 6 to 8 hours.
[0031] The general structural formula of the green and environmentally friendly gold leaching agent mentioned above In the case of R 1 and R 2 When both are Cl, the gold leaching agent is A-1; when R 1 Cl, R 2 When it is H, the gold immersion agent is A-2; when R 1 For H, R 2 When it is Cl, the gold leaching agent is A-3; when R 1 and R 2 When both are Br, the gold leaching agent is A-4; when R 1 Br, R 2 When it is H, the gold immersion agent is A-5; when R 1 For H, R 2 When Br, the gold leaching agent is A-6; when R 1 Cl, R 2 When Br, the gold leaching agent is A-7; when R 1 Br, R 2 When it is Cl, the gold leaching agent is A-8.
[0032] Specifically, A-1 is A-2 is A-3 is A-4 is A-5 is A-6 A-7 is A-8
[0033] The preparation method of A-7 is as follows: 1 mol of cyanuric acid is prepared into a slurry with deionized water, the pH value of the slurry system is maintained at 3 to 4 with 3M hydrochloric acid, 2.5 to 3.5 mol of hypochlorous acid solution is added at room temperature, and the reaction is carried out for 2 to 3 hours. After the reaction is completed, a vacuum water pump is used to evacuate the chlorine gas that has not reacted completely, and then the pressure is restored to normal, dimethyl sulfoxide is added and stirred at 40 to 50° C. for 1 hour, filtered, the filtered solution is collected, deionized water is added, and the precipitated solid is collected by filtration, the precipitated solid is prepared into a slurry with deionized water, 1.5 to 2 mol of sodium bromate is added, the pH value of the slurry system is maintained at 3 to 4 with 3M hydrochloric acid, and the reaction is carried out for 2 to 3 hours at room temperature. After the reaction is completed, the slurry is heated at 100° C. and refluxed for 20 to 30 minutes to promote the decomposition of hydrobromic acid, and finally, the product gold leaching agent A-7 (dichloro, monobromoisocyanuric acid) is collected by vacuum distillation.
[0034] The process for treating acidic gold-containing minerals provided by the present invention is described below in conjunction with specific embodiments.
[0035] Example 1
[0036] Example 1 provides a process for treating acidic gold-containing minerals. The acidic gold-containing material used in the test is biological oxidation slag, and the multi-element content of the ore is shown in Table 1 below:
[0037] Table 1 Multi-element analysis of biological oxidation slag
[0038] Element Au* Ag* S As Fe Cu Ca Pb Zn content(%) 35.15 1.22 2.25 3.11 9.40 0.15 2.50 0.19 1.35
[0039] Note: *Unit is g / t;
[0040] The specific processing process includes the following steps:
[0041] S1. Preparation of slurry: Take 500g of acidic gold-containing material, add water and ball mill for 25min, crush it to the ore powder with a particle size of -0.074mm, which accounts for 80% of the total mass of the material, pour the ball-milled ore powder into a stirring tank, add water under mechanical stirring to adjust the slurry concentration to 30%;
[0042] S2. Add green and environmentally friendly gold leaching agent A-1 to the ore pulp prepared in step S1, and the concentration of A-1 is 0.1 mol / L.
[0043] S3. Add dilute hydrochloric acid to adjust the pH value of the slurry to 2, stir at room temperature for 6 hours, and leach gold.
[0044] Example 2
[0045] Example 2 provides a process for treating acidic gold-containing minerals. Compared with Example 1, the difference is that the gold-containing material used is a flotation gold concentrate, and the multi-element content of the ore is shown in Table 2 below. The remaining experimental parameters and conditions are basically the same as those in Example 1 and are not repeated here.
[0046] Table 2 Multi-element analysis of a flotation gold concentrate
[0047] Element Au* Zn S As Fe Cu Ca C <![CDATA[SiO 2 ]]> content(%) 25.25 2.52 0.30 1.15 12.50 1.19 3.50 0.39 36.91
[0048] Note: *Unit is g / t;
[0049] Embodiment 3-9
[0050] Examples 3-9 respectively provide a process for treating acidic gold-containing minerals. Compared with Example 1, the difference is that the type of gold leaching agent added in step S2 is different, as shown in Table 3. The remaining experimental parameters and conditions are basically the same as those in Example 1 and will not be repeated here.
[0051] The gold leaching rates in Examples 1-9 are shown in the following table.
[0052] Table 3 Gold leaching rate of Examples 1-9
[0053]
[0054]
[0055] Note: The detection error is ±2%.
[0056] As shown in Table 3, the gold leaching rates of Examples 1-2 show that the green-environmentally friendly gold leaching agent has good applicability to different types of acidic gold-containing minerals. As shown in the gold leaching rates of Examples 1-9, the green-environmentally friendly gold leaching agent can achieve efficient gold leaching in an acidic environment.
[0057] Examples 10-11 and Comparative Examples 1-2
[0058] Examples 10-11 and Comparative Examples 1-2 respectively provide a process for treating acidic gold-containing minerals. Compared with Example 1, the difference is that in step S2, the concentration of the green-environmentally friendly gold leaching agent in the slurry is different, as shown in Table 4. The remaining experimental parameters and conditions are basically the same as those in Example 1 and are not repeated here.
[0059] The gold leaching rates of Examples 10-11 and Comparative Examples 1-2 are shown in the following table.
[0060] Table 4 Gold leaching rate of Examples 10-11 and Comparative Examples 1-2
[0061] project Gold leaching agent concentration (mol / L) Gold leaching rate (%) Example 1 0.1 96 Example 10 0.05 94 Embodiment 11 0.2 96 Comparative Example 1 0.04 91 Comparative Example 2 0.21 96
[0062] Note: The detection error is ±2%.
[0063] It can be seen from Table 4 that there is an optimal range for the dosage of green-environmentally friendly gold leaching agents. When the dosage is below this range, the gold leaching rate is low and the leaching effect is poor. When the dosage exceeds the range, the leaching effect will no longer be significantly improved.
[0064] Examples 12-14 and Comparative Examples 3-4
[0065] Examples 12-14 and Comparative Examples 3-4 respectively provide a process for treating acidic gold-containing minerals. Compared with Example 1, the difference is that in step S3, the pH value of the slurry is adjusted differently, as shown in Table 5. The remaining experimental parameters and conditions are basically the same as those in Example 1 and will not be repeated here.
[0066] Table 5 Gold leaching rate of Examples 12-14 and Comparative Examples 3-4
[0067] project Slurry pH Gold leaching rate (%) Example 1 2 96 Example 12 1 96 Embodiment 13 3 96 Embodiment 14 4 94 Comparative Example 3 5 83 Comparative Example 4 6 72
[0068] Note: The detection error is ±2%.
[0069] As can be seen from Table 5, the gold leaching rates of Examples 12-14 and Comparative Examples 3-4 show that the optimal applicable pH of the green-environmentally friendly gold leaching agent is 1-4. As the acidity of the leaching system decreases, when the pH>4, the gold leaching effect deteriorates. The reasons can be summarized as follows: when the pH increases, the hydrolysis rate of the halogenated derivatives of isocyanuric acid is too fast, and it is also accompanied by a large number of side reactions. A series of negative factors lead to the deterioration of the gold leaching effect.
[0070] In summary, in the gold leaching process of the present invention, the halogenated derivatives of isocyanuric acid play a dual role as an oxidant and a complexing agent. For example, when the halogenated derivative of isocyanuric acid is chloroisocyanuric acid, chloroisocyanuric acid can be mildly hydrolyzed to release high-valent chlorine (ClO - ), positive monovalent chloride (chloroisocyanuric acid, hypochlorite) and negative monovalent chloride ion (Cl - ) forms a redox potential pair, which maintains the potential stability of the system. In the process of chlorine reduction, gold can be oxidized, and the formed gold ions (III) can form extremely stable gold complexes with chloride ions. The consumption of chloride ions promotes the positive transformation of hypochlorite to chloride ions, and the consumption of hypochlorite further promotes the hydrolysis of chloroisocyanuric acid. Through a series of reactions of halogenated derivatives of isocyanuric acid, the chemical equilibrium is progressively carried out layer by layer, and finally the efficient leaching of gold is achieved. The entire process does not require acid-base transformation, and has excellent leaching effect under leaching conditions of normal temperature and pressure. The reagent system is cyanide-free, environmentally friendly, and efficient, and has poor corrosion to stainless steel leaching equipment, achieving the balance between environmental protection and economy to the greatest extent.
[0071] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A process for treating acidic gold-bearing minerals, It is characterized in that The following steps are involved: S1. crushing the acidic gold-containing material, adding water to adjust the slurry to a mass percentage concentration of the slurry within a predetermined range; S2. Add one or more green-environmentally friendly gold leaching agents to the slurry to make the green-environmentally friendly gold leaching agent reach a preset concentration; the green-environmentally friendly gold leaching agent is one or more halogenated derivatives of isocyanuric acid, and its general structural formula is In the formula, R 1 and R 2 Respectively represent one of Cl, Br and H; S3. Add a pH adjuster to adjust the pH value of the slurry to a predetermined range, stir for a predetermined time at room temperature, and leach gold.
2. The process for treating acidic gold-bearing minerals according to claim 1, It is characterized in that In step S1, the acidic gold-containing material includes one or more of biological oxidation slag, biological oxidation heap leaching slag, sulfuric acid slag, roasted sand and flotation gold concentrate.
3. The process for treating acidic gold-containing minerals according to claim 2, It is characterized in that The crushing process is to crush the material to a size of -0.074 mm, wherein the ore powder accounts for 75% to 85% of the total mass of the material.
4. The process for treating acidic gold-bearing minerals according to claim 2, It is characterized in that The concentration of the ore pulp is 30% to 35%.
5. The process for treating acidic gold-bearing minerals according to claim 1, It is characterized in that In step S2, in the general structural formula of the green-environmentally friendly gold leaching agent, when R 1 When it is Cl, R 2 is Cl or H or Br; when R 1 When H, R 2 is Cl or Br; when R 1 When Br, R 2 It is Cl or H or Br.
6. The process for treating acidic gold-bearing minerals according to claim 1, It is characterized in that In step S2, the concentration of the green and environmentally friendly gold leaching agent is 0.05-0.2 mol / L.
7. The process for treating acidic gold-bearing minerals according to claim 1, It is characterized in that In step S3, the pH adjuster is dilute hydrochloric acid.
8. The process for treating acidic gold-bearing minerals according to claim 7, It is characterized in that The predetermined range of pH value of the slurry is 1-4.
9. The process for treating acidic gold-bearing minerals according to claim 7, It is characterized in that The stirring time is 6 to 8 hours.