Method for smelting magnesium from serpentine and comprehensively utilizing serpentine
By using a combined process of serpentine, silicon-aluminum-calcium alloy and silicon nanowires in magnesium smelting, magnesium extraction and valuable component recovery are optimized, and the problems of carbon emissions and slag reuse in magnesium smelting are solved, achieving high efficiency, Environmentally friendly magnesium production process.
Patent Information
- Application Number
- CN202410986113.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing magnesium smelting technology has low single furnace output, large area, low degree of automation, and large greenhouse gas emissions. In particular, the carbon emissions are huge during dolomite calcination, and the magnesium slag cannot be reused, resulting in environmental pollution.
Using serpentine as raw material, using a combined reducing agent of silicon-aluminum-calcium alloy and silicon nanowires, combined with negative pressure magnesium synthesis technology, optimizes the reaction activity and physical chemical characteristics of magnesium synthesis, builds microscopic conduction paths, reduces energy consumption and carbon emissions, And the recycling of valuable components is achieved through magnetic separation and carbon reduction smelting.
It improves the magnesium extraction efficiency, realizes efficient recycling of valuable ingredients, reduces the comprehensive energy consumption and carbon emissions of the magnesium refining process, avoids waste emissions, and has significant environmental benefits.
Smart Images

Figure BDA0004957440610000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal smelting, and in particular relates to a novel method for smelting magnesium with serpentine and its comprehensive utilization. Background Art
[0002] As a lightweight structural material and functional material, magnesium metal will play an important role in promoting green, low-carbon and high-quality development and show greater achievements. The smelting of raw magnesium is mainly based on thermal methods. The main process for extracting raw magnesium uses dolomite as raw material and adopts the Pijiang method. The production process includes dolomite calcination, silicon thermal reduction and refining process. However, there are currently low single furnace output, large floor space, low degree of automation, and high greenhouse gas emissions. In particular, a large amount of CO2 will be directly emitted during the calcination of dolomite. For every ton of magnesium produced, 4 to 5 tons of carbon emissions will be generated during the calcination process. It can be seen that the carbon emissions are huge. Moreover, 1 ton of magnesium will produce 6 to 7 tons of reduced slag. The residue contains a high amount of magnesium, and the slag cannot be reused in building materials, making the slag an industrial waste and seriously polluting the environment.
[0003] Serpentine is a new raw material for magnesium smelting. Using serpentine to smelt magnesium can avoid carbon emissions from calcining dolomite, and can effectively solve the problem of resource utilization of asbestos tailings. At present, there have been a small number of studies in this area. For example, the patent "Method for preparing metallic magnesium and byproducts by vacuum carbon thermal reduction of serpentine minerals" (CN101560603B) discloses a method for smelting magnesium using serpentine as a raw material and using carbon thermal reduction, but its processing temperature reaches 1200-1500°C. The reduction tank currently used is easily deformed and damaged at this high temperature, so it is not suitable for large-scale industrial application. The patent "A method for preparing metallic magnesium, silicon, nickel and iron using serpentine ore and / or asbestos tailings" (CN115818686 A) discloses a method of first treating serpentine with microwave alkali fusion, and then using microwave method to reduce the alkali slag to extract magnesium. This method has certain innovation, but microwave treatment is not only costly and difficult to accurately control the temperature, but also high-temperature alkali fusion seriously corrodes the equipment, and it is not suitable for large-scale industrial application. How to propose a method that is more suitable for practical application, to efficiently extract magnesium from serpentine, and to comprehensively recover the valuable components contained therein is a problem that needs to be solved urgently. Summary of the invention
[0004] In order to realize the efficient extraction of magnesium from serpentine and the comprehensive recovery and utilization of valuable components, the present invention provides a novel method for smelting magnesium from serpentine and its comprehensive utilization.
[0005] A serpentine magnesium smelting method, wherein a mixture of serpentine, a reducing agent, silicon nanowires and an additive is subjected to magnesium smelting treatment at a temperature of 1000 to 1200° C., and metallic magnesium and magnesium smelting slag are collected;
[0006] The reducing agent is a silicon-aluminum-calcium alloy;
[0007] The auxiliary agent is metal fluoride.
[0008] The innovative research of the present invention shows that the use of the silicon-aluminum-calcium alloy as a reducing agent, in combination with the silicon nanowires, can enhance the magnesium smelting reaction activity of serpentine. In addition, it is also helpful to optimize the physical and chemical characteristics of the reduction stage, such as constructing a microscopic conductive path and a regional reaction microcavity, which is helpful for the extraction of magnesium. In addition, it is also beneficial to the circulation of materials, low-temperature magnesium smelting, and its cyclic magnesium smelting performance.
[0009] In the present invention, the content of Si, Al and Ca in the silicon-aluminum-calcium alloy is 5-50:50-95:1-20, and can further be 5-30:55-85:5-15. The alloy particle size is 300-1000 mesh.
[0010] In the present invention, the auxiliary agent includes CaF 2 MgF 2 , AlF 3 At least one of .
[0011] In the present invention, the mixture is pellets, which are obtained by crushing serpentine and mixing it with a reducing agent, silicon nanowires and an additive, and then pressing and molding it;
[0012] Preferably, the aspect ratio of the silicon nanowire is above 50, further 50 to 300, and further 80 to 210. Studies have shown that under the preferred aspect ratio, the physical and chemical characteristics of the magnesium smelting reaction can be further optimized, the efficiency and effect of magnesium smelting can be further optimized, and energy consumption and carbon dioxide emissions can be reduced.
[0013] Preferably, the median value of the diameter D of the silicon nanowire is 100-200 nm, and the length L is ≥10 μm.
[0014] Preferably, the particle size of the serpentine is 300-500 mesh;
[0015] Preferably, the weight ratio of serpentine, reducing agent, silicon nanowires, and auxiliary agent is 100:20-80:0.5-2:1-3;
[0016] Preferably, the pressure of the pressing molding is 50 to 100 MPa;
[0017] Preferably, the particles of the mixture are 2 to 10 cm.
[0018] In the present invention, the pressure of the magnesium smelting process is negative pressure, and further can be below 100 Pa;
[0019] Preferably, the magnesium smelting time is more than 2 hours, and can be further extended to 5 to 20 hours in consideration of efficiency.
[0020] The present invention also provides a method for comprehensive utilization of serpentine, wherein the method described in the present invention is used to carry out magnesium smelting treatment on serpentine to obtain metallic magnesium and magnesium smelting slag; and the magnesium smelting slag is subjected to magnetic separation treatment to obtain nickel-iron magnetic separation components and magnetic separation slag.
[0021] In the present invention, the magnetic separation intensity is 10000 to 20000 Gauss.
[0022] The present invention also includes the step of reducing and smelting the magnetic separation slag to obtain the silicon-aluminum-calcium alloy.
[0023] In the present invention, a carbonaceous reducing agent is selected in the reduction smelting stage;
[0024] Preferably, the carbonaceous reducing agent comprises at least one of bituminous coal, charcoal, petroleum coke and washed coal;
[0025] Preferably, the weight ratio of the magnetic separation slag to the carbonaceous reducing agent is 100:20-50;
[0026] Preferably, the temperature of reduction smelting is 1800-2100°C;
[0027] Preferably, the reduction smelting time is 2 to 10 hours.
[0028] In the present invention, silicon-aluminum-calcium alloy is used as a reducing agent and is cyclically used in the magnesium smelting process of serpentine.
[0029] The process described in the present invention can unexpectedly achieve high-activity cyclic regeneration of the reducing agent.
[0030] Beneficial effects:
[0031] The present invention can optimize the physical and chemical characteristics of magnesium reduction of serpentine by combining the ternary alloy reducing agent and silicon nanowires, and can optimize the magnesium reaction activity. In addition, the reaction microstructure can be optimized, and a three-dimensional conductive network can be constructed to improve the magnesium refining effect and significantly improve the magnesium extraction efficiency. This process can realize the circulation of reducing agents for magnesium refining and realize the efficient recovery of valuable elements in serpentine ore, and is a high-value comprehensive utilization process. In addition, the whole process basically has no waste discharge, avoiding the problem that traditional magnesium smelting slag cannot be handled, greatly reducing the comprehensive energy consumption and carbon emissions of the entire magnesium refining process, and has significant environmental benefits. DETAILED DESCRIPTION
[0032] The present invention will be described in detail below with reference to the embodiments, but the present invention is not limited thereto.
[0033] An optional serpentine comprehensive utilization step of the present invention includes, for example, the following steps:
[0034] ① Use jaw crusher, roller crusher and air flow mill respectively to crush and grind serpentine into particles of 300-500 mesh.
[0035] ② Mix the crushed serpentine with the alloy reducing agent - silicon aluminum calcium alloy powder, silicon nanowires, and additives. The weight ratio of serpentine to silicon aluminum calcium alloy is 100:20-80; the content of Si, Al, and Ca in the silicon aluminum calcium alloy is 5-50:50-95:1-20, respectively, and the alloy particle size is 300-1000 mesh. The median diameter of the silicon nanowire is 100-200nm, the length is ≥10μm, the aspect ratio is 80-210, and the weight ratio with serpentine is 100:0.5-2. The additive is mainly CaF 2 MgF 2 , AlF 3 etc., the weight ratio of the additive to serpentine is 100:1-3.
[0036] ③ The mixed powder is pressed into pellets on a pellet press at a pressure of 50-100 MPa and a particle size of 2-10 cm. The pressed pellets are then placed in a magnesium reduction tank for reaction at a temperature of 1000-1200°C, a pressure in the tank below 100 Pa, and a reaction time of more than 2 hours, further 5-20 hours. After the reaction, the temperature is lowered and the vacuum is broken, and metallic magnesium can be collected in a crystallizer.
[0037] ④ The magnesium smelting slag after the above reaction is placed in a dry electromagnetic magnetic separator for treatment, and the magnetic induction intensity is 10000-20000 Gauss. Repeat the treatment 3 times, and after magnetic separation, nickel-iron components and magnetic separation slag are obtained.
[0038] ⑤ Mix the magnetic separation slag with a carbon reducing agent, such as bituminous coal, charcoal, petroleum coke, washed coal, etc. The weight ratio of magnetic separation powder to carbon reducing agent is 100:20-50. After mixing, put it into a submerged arc furnace for reaction at a reaction temperature of 1800-2100°C, an argon atmosphere, and a reaction time of 2-10 hours. During the reaction, a silicon-aluminum-calcium alloy liquid will be obtained, which will be cooled to obtain an alloy ingot.
[0039] ⑥ The silicon-aluminum-calcium alloy ingot obtained above is used as a reducing agent and recycled for the magnesium smelting process in step ②.
[0040] The following is a specific plan:
[0041] Example 1
[0042] ① Use jaw crusher, roller crusher and air flow mill to crush and grind serpentine into particles of 300-500 mesh. Mix the crushed serpentine with alloy reducing agent - silicon aluminum calcium alloy powder, silicon nanowire and additives. The weight ratio of serpentine to silicon aluminum calcium alloy is 100:50; the weight ratio of Si, Al and Ca in the silicon aluminum calcium alloy is 30:55:15, and the alloy particle size is 325 mesh. The median diameter of silicon nanowire is 120nm, the length is 10-15μm, the aspect ratio is 90, and the weight ratio with serpentine is 100:1.5. The additive is mainly AlF3, and the weight ratio of additive to serpentine is 100:3.
[0043] ② Press the mixed powder into pellets on a pellet press at a pressure of 50MPa and a particle size of 2cm. Then put the pressed pellets into a magnesium reduction tank for reaction at a temperature of 1000℃, a pressure in the tank below 20Pa, and a reaction time of 5h. After the reaction, cool down and break the vacuum, and metal magnesium can be collected in the crystallizer.
[0044] ③ The magnesium smelting slag after the above reaction is placed in a dry electromagnetic magnetic separator for treatment, and the magnetic induction intensity is 10,000 Gauss. Repeat the process 3 times to obtain nickel-iron magnetic components and magnetic separation powder (magnetic separation slag) after magnetic separation. The above magnetic separation powder is mixed with a carbon reducing agent, the carbon reducing agent is bituminous coal, and the weight ratio of magnetic separation powder to carbon reducing agent is 100:50. After mixing, put it into a submerged arc furnace for reaction, the reaction temperature is 2100°C, the atmosphere is argon, and the reaction time is 2.5h. During the reaction, a silicon-aluminum-calcium alloy liquid will be obtained, and after cooling it, an alloy ingot will be obtained.
[0045] ④ Test the element content of the silicon-aluminum-calcium alloy ingot obtained above, then perform high-temperature smelting, and according to the composition of the alloy reducing agent in step ①, add the corresponding elements to obtain an alloy ingot with the same composition of the alloy reducing agent, and then crush it into the alloy reducing agent.
[0046] Example 2
[0047] ① Use jaw crusher, roller crusher and air flow mill to crush and grind serpentine into particles of 300-500 mesh. Mix the crushed serpentine with alloy reducing agent - silicon aluminum calcium alloy powder, silicon nanowire and additives. The weight ratio of serpentine to silicon aluminum calcium alloy is 100:75; the content of Si, Al and Ca in the silicon aluminum calcium alloy is 20:75:5 respectively, and the alloy particle size is 600 mesh. The median diameter of silicon nanowire is 150nm, the length is 15-20μm, the aspect ratio is 125, and the weight ratio with serpentine is 100:1. The additive is mainly MgF2, and the weight ratio of additive to serpentine is 100:2.
[0048] ② Press the mixed powder into pellets on a pellet press at a pressure of 75MPa and a particle size of 5cm. Then put the pressed pellets into a magnesium reduction tank for reaction at a temperature of 1100℃, a pressure in the tank below 20Pa, and a reaction time of 10h. After the reaction, cool down and break the vacuum, and metal magnesium can be collected in the crystallizer.
[0049] ③ The magnesium smelting slag after the above reaction is placed in a dry electromagnetic separator for treatment, and the magnetic induction intensity is 150,000 Gauss. Repeat the process 3 times to obtain nickel-iron magnetic components and magnetic separation powder (magnetic separation slag) after magnetic separation. The above magnetic separation powder is mixed with a carbon reducing agent, the carbon reducing agent is charcoal, and the weight ratio of magnetic separation powder to carbon reducing agent is 100:35. After mixing, put it into a submerged arc furnace for reaction, the reaction temperature is 1950°C, the atmosphere is argon, and the reaction time is 7.5h. During the reaction, a silicon-aluminum-calcium alloy liquid will be obtained, and after cooling it, an alloy ingot will be obtained.
[0050] ④ Test the element content of the silicon-aluminum-calcium alloy ingot obtained above, then perform high-temperature smelting, and according to the composition of the alloy reducing agent in step ①, add the corresponding elements to obtain an alloy ingot with the same composition of the alloy reducing agent, and then crush it into the alloy reducing agent.
[0051] Example 3
[0052] ① Use jaw crusher, roller crusher and air flow mill to crush and grind serpentine into particles of 300-500 mesh. Mix the crushed serpentine with alloy reducing agent - silicon aluminum calcium alloy powder, silicon nanowire and additives. The weight ratio of serpentine to silicon aluminum calcium alloy is 100:25; the content of Si, Al and Ca in the silicon aluminum calcium alloy is 5:85:10 respectively, and the alloy particle size is 800 mesh. The median diameter of silicon nanowire is 195nm, the length is 30-40μm, the aspect ratio is 200, and the weight ratio with serpentine is 100:0.6. The additive is mainly CaF2, and the weight ratio of additive to serpentine is 100:1.
[0053] ② Press the mixed powder into pellets on a pellet press at a pressure of 100MPa and a particle size of 10cm. Then put the pressed pellets into a magnesium reduction tank for reaction at a temperature of 1200℃, a pressure in the tank below 50Pa, and a reaction time of 20h. After the reaction, cool down and break the vacuum, and metal magnesium can be collected in the crystallizer.
[0054] ③ The magnesium smelting slag after the above reaction is placed in a dry electromagnetic separator for treatment, and the magnetic induction intensity is 20,000 Gauss. Repeat the process three times to obtain nickel-iron magnetic components and magnetic powder (magnetic slag) after magnetic separation. The magnetic powder is mixed with a carbon reducing agent, the carbon reducing agent is petroleum coke, and the weight ratio of magnetic powder to carbon reducing agent is 100:25. After mixing, put it into a submerged arc furnace for reaction, the reaction temperature is 1800°C, the atmosphere is argon, and the reaction time is 10h. During the reaction, a silicon-aluminum-calcium alloy liquid will be obtained, and after cooling it, an alloy ingot will be obtained.
[0055] ④ Test the element content of the silicon-aluminum-calcium alloy ingot obtained above, then perform high-temperature smelting, and according to the composition of the alloy reducing agent in step ①, add the corresponding elements to obtain an alloy ingot with the same composition of the alloy reducing agent, and then crush it into the alloy reducing agent.
[0056] Example 4
[0057] Compared with Example 1, the only difference is that in step ④, the silicon-aluminum-calcium alloy ingot obtained above is smelted with metal aluminum particles and calcium particles according to the ratio of the reducing agent in Example 1 (the weight ratio of Si, Al, Ca is 30:55:15) to obtain a regenerated alloy reducing agent, which is recycled to step ① to participate in the subsequent serpentine treatment.
[0058] Example 5
[0059] Compared with Example 1, the only difference is that the silicon nanowires with a length of 5-8 μm and an aspect ratio of 50 are used, and the silicon nanowires are replaced by equal weight. Other operations and parameters are the same as in Example 1.
[0060] Example 6
[0061] Compared with Example 1, the only difference is that the silicon nanowires with a length of 35-40 μm and an aspect ratio of 300 are used, and the silicon nanowires are replaced by equal weight. Other operations and parameters are the same as in Example 1.
[0062] Comparative Example 1
[0063] Compared with Example 1, the only difference is that the type of reducing agent is changed, specifically:
[0064] Group A: The reducing agent is a silicon-aluminum alloy lacking Ca, and the weight of the remaining silicon-aluminum is the same as in Example 1, and the total amount of the reducing agent is the same as in Example 1.
[0065] Group B: The reducing agent is a silicon-aluminum alloy, and a small amount of Ca or other calcium elements such as CaO are supplemented. The other operating conditions such as the element ratio of silicon, aluminum and calcium in the reducing agent and the total element dosage are the same as those in Example 1.
[0066] Group C: The reducing agent is a silicon-calcium alloy lacking Al, and the weight of the remaining silicon-calcium is the same as that in Example 1, and the total amount of the reducing agent is the same as that in Example 1.
[0067] Comparative Example 2
[0068] Compared with Example 1, the only difference is that the silicon nanowires are missing, and other operations and parameters are the same as Example 1.
[0069] Comparative Example 3
[0070] Compared with Example 1, the only difference is that silicon nanoparticles (D50 is 120 nm) of equal weight are used to replace the silicon nanowires, and other operations and parameters are the same as Example 1.
[0071] Table 1
[0072]
[0073] As can be seen from Table 1, the process described in the present invention can optimize the extraction effect of magnesium, and can also effectively reduce emissions and energy consumption. In addition, the present invention also shows that through Example 4, the magnesium extraction rate after 5 cycles can still be obtained above 90%, with excellent reductant regeneration catalytic stability.
Claims
1. A method for smelting magnesium from serpentine, It is characterized in that The mixture of serpentine, reducing agent, silicon nanowires and additives is subjected to magnesium smelting treatment at a temperature of 1000-1200° C., and metallic magnesium and magnesium smelting slag are collected; The reducing agent is a silicon-aluminum-calcium alloy; The auxiliary agent is metal fluoride.
2. The serpentine magnesium smelting method according to claim 1, It is characterized in that In the silicon-aluminum-calcium alloy, the contents of Si, Al and Ca are 5-50:50-95:1-20.
3. The serpentine magnesium smelting method according to claim 1, It is characterized in that The additives include CaF 2 MgF 2 , AlF 3 At least one of .
4. The serpentine magnesium smelting method according to claim 1, It is characterized in that The mixture is pellets, which are obtained by crushing serpentine and mixing it with a reducing agent, silicon nanowires and an additive, and then pressing and molding it; Preferably, the aspect ratio of the silicon nanowire is greater than 50, further 50 to 300; further 80 to 210; Preferably, the diameter of the silicon nanowire is 100-200 nm and the length is ≥10 μm; Preferably, the particle size of the serpentine is 300-500 mesh; Preferably, the weight ratio of serpentine, reducing agent, silicon nanowires, and auxiliary agent is 100:20-80:0.5-2:1-3; Preferably, the pressure of the pressing molding is 50 to 100 MPa; Preferably, the particles of the mixture are 2 to 10 cm.
5. The serpentine magnesium smelting method according to claim 1, It is characterized in that The pressure of magnesium smelting treatment is below 100Pa; Preferably, the magnesium smelting time is 2 hours or more, and further 5 to 20 hours.
6. A method for comprehensive utilization of serpentine, It is characterized in that The method according to any one of claims 1 to 5 is used to carry out magnesium smelting treatment on serpentine to obtain metallic magnesium and magnesium smelting slag; the magnesium smelting slag is subjected to magnetic separation treatment to obtain nickel-iron magnetic separation components and magnetic separation slag.
7. The serpentine comprehensive utilization method according to claim 6, It is characterized in that The magnetic separation intensity is 10000-20000 Gauss.
8. The serpentine comprehensive utilization method according to claim 6 or 7, It is characterized in that The method also includes the step of reducing and smelting the magnetic separation slag to obtain the silicon-aluminum-calcium alloy.
9. The serpentine comprehensive utilization method according to claim 8, It is characterized in that The reduction smelting stage uses a carbonaceous reducing agent; Preferably, the carbonaceous reducing agent comprises at least one of anthracite, charcoal, petroleum coke and clean coal; Preferably, the weight ratio of the magnetic separation slag to the carbonaceous reducing agent is 100:20-50; Preferably, the temperature of reduction smelting is 1800-2100°C; Preferably, the reduction smelting time is 2 to 10 hours.
10. The serpentine comprehensive utilization method according to claim 8 or 9, It is characterized in that The silicon-aluminum-calcium alloy is used as a reducing agent in the method according to any one of claims 1 to 5 and is cyclically used in the magnesium smelting process of serpentine.
Citation Information
Patent Citations
Method for preparing magnesium metal and by-product by vacuum carbothermic reduction with serpentine minerals
CN101560603B
Method for preparing magnesium, silicon, nickel and iron from serpentine ore and / or asbestos tailings
CN115818686A