Antioxidant aluminum alloy additive and preparation method thereof

Through the combination of magnesium-aluminum alloy powder, modified carbon powder, composite metal powder and additives and nozzle atomization technology, anti-oxidation aluminum alloy additives are prepared, which solves the oxidation problem of aluminum alloy materials in humid environments and significantly improves its resistance Oxidation and corrosion resistance, suitable for complex environments.

CN118932198AInactive Publication Date: 2024-11-12GUANGYA ALUMINUM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997289.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure BDA0004960594490000061
    Figure BDA0004960594490000061
  • Figure BDA0004960594490000071
    Figure BDA0004960594490000071
  • Figure BDA0004960594490000072
    Figure BDA0004960594490000072
Patent Text Reader

Abstract

The invention discloses an antioxidant aluminum alloy additive and a preparation method thereof, and belongs to the field of aluminum alloy preparation. The antioxidant aluminum alloy additive comprises, by weight, magnesium-aluminum alloy powder, modified carbon powder, composite metal powder and auxiliaries, wherein the composite metal powder is composed of Ni, Pb, Re, Cr and Be according to the mass ratio of (1-3): (2-7): (1-7): (1-3): (1-2). After the magnesium-aluminum alloy powder, the modified carbon powder, the composite metal powder and the auxiliaries are compounded, the specific components interact, the performance of the aluminum alloy material is guaranteed, meanwhile, generated bubbles can be reduced, the crystal lattice size can be reduced, compactness is improved, and the service life of the aluminum alloy material is prolonged. The whole anti-oxidation effect is obviously promoted, so that the antioxidant composition is suitable for more complex use environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of aluminum alloy preparation, and in particular to an anti-oxidation aluminum alloy additive and a preparation method thereof. Background Art

[0002] Aluminum alloy has the characteristics of light weight, good toughness, corrosion resistance and unique metallic luster. It is adopted by more and more electronic appliances, communication equipment, lighting devices, automobiles and other parts, such as the shells of smart phones, laptops, tablet computers, radiators and lampshades of LED lights, radiators, cabinets, filters of 3G and 4G wireless communication base stations, heating plates of rice cookers, induction cookers, water heaters, controller chassis and drive motor shells of new energy vehicles. In order to meet the needs of thin-walled, lightweight, high-strength and casting production of parts, higher and higher requirements are put forward for the casting fluidity and mechanical properties of aluminum alloys. Although the surface of aluminum alloy profiles or plates used in the market is treated with anti-oxidation, the anti-oxidation protective film or protective layer will not only greatly increase the production cost, but also the anti-oxidation effect cannot reach the ideal state. For example, it is used in a humid environment with relatively large acidity and alkalinity such as a bathroom, because in a humid environment, aluminum alloy materials often oxidize and turn yellow and black, and even in a dry indoor environment, the service life is not satisfactory. In order to improve the user experience, the existing technology only improves the corrosion resistance of aluminum alloy materials. For example, Chinese invention patent CN 109088184A discloses a titanium-clad aluminum alloy corrosion-resistant grounding material; it is a layer of metal titanium coated on the surface of the inner aluminum alloy material, wherein the mass percentage of each component of the inner aluminum alloy material is: C5-10%, Cu 5-8%, Si <1.5%, rare earth 0.05-0.1%; the grounding material can not only ensure the original conductivity of the aluminum alloy, but also protect the aluminum alloy from corrosion by covering with titanium, and can cope with the corrosion caused by highly corrosive soil media, meeting the use requirements of the grounding material corrosion resistance, but the preparation process is complicated, the raw materials and manufacturing costs are high, and it is difficult to be widely used. However, the tensile properties of the aluminum alloy obtained are general, and the oxidation resistance is poor, which still cannot meet the long-term use in complex and harsh environments. Therefore, it is necessary to develop a material that can enhance the oxidation resistance of aluminum alloys to meet market demand. Summary of the invention

[0003] Based on this, in order to solve the problem of poor oxidation resistance of aluminum alloy in the prior art, the present invention provides an antioxidant aluminum alloy additive and a preparation method thereof, and the specific technical scheme is as follows:

[0004] An antioxidant aluminum alloy additive, the antioxidant aluminum alloy additive comprising the following preparation raw materials in parts by weight:

[0005] 22 to 30 parts of magnesium aluminum alloy powder, 7 to 13 parts of modified carbon powder, 9 to 15 parts of composite metal powder, and 1 to 7 parts of additives;

[0006] The composite metal powder is composed of Ni, Pb, Re, Cr and Be in a mass ratio of (1-3): (2-7): (1-7): (1-3): (1-2).

[0007] Furthermore, it is characterized in that the auxiliary agent is at least one of cerium dioxide, boron carbide and silicon nitride.

[0008] In addition, the present application also provides a method for preparing an oxidation-resistant aluminum alloy additive, the preparation method comprising the following steps:

[0009] Add the carbon powder to ethanol, stir for 1 h to 2 h, let stand for 10 min to 25 min, filter, wash the filter cake repeatedly with water, and dry to obtain modified carbon powder;

[0010] Magnesium-aluminum metal powder, composite metal powder and additives are added to a mixing kettle for the first smelting treatment, and then modified carbon powder is added for a second smelting treatment. The jet passes through the nozzle component and meets the atomizing medium, and is dispersed into metal droplets under the action of the atomizing medium. The component powder is cooled and solidified to obtain an antioxidant aluminum alloy additive.

[0011] Furthermore, the solid-liquid ratio of the carbon powder to ethanol is 1 g / (15-20) mL.

[0012] Furthermore, the drying process is carried out at a temperature of 65° C. to 95° C. and for a time of 20 min to 60 min.

[0013] Furthermore, the temperature of the first smelting treatment is 900° C. to 1500° C., the vacuum degree is 25 Pa to 35 Pa, and the time is 35 min to 55 min.

[0014] Furthermore, the temperature of the second smelting treatment is 1200° C. to 1250° C., the atomization pressure is 0.5 MPa to 1.0 MPa, and the time is 20 min to 35 min.

[0015] Furthermore, after the second smelting treatment, ultrasonic treatment is required for 10 minutes to 20 minutes, and the power of the ultrasonic treatment is 100W to 150W.

[0016] Furthermore, the flow rate of the jet is 1 L / min to 3 L / min.

[0017] Furthermore, the average particle size of the anti-oxidation aluminum alloy additive is 50 μm to 120 μm.

[0018] In the above scheme, after the magnesium-aluminum alloy powder, modified carbon powder, composite metal powder and additives are compounded, the specific components interact with each other, while ensuring the performance of the aluminum alloy material, the material's antioxidant ability can be effectively improved, making it suitable for more complex use environments. Specifically, the modified carbon powder matrix can effectively prevent oxygen atoms from diffusing to the surroundings, and the oxidation value is low. The magnesium-aluminum alloy powder not only has a bonding effect, but also acts as a carrier for uniformly dispersing the modified carbon powder. In combination with the composite metal powder and additives, the synergistic effect can reduce the generation of bubbles and the lattice size, increase the density, and significantly promote the overall antioxidant effect. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0021] An antioxidant aluminum alloy additive in one embodiment of the present invention comprises the following raw materials in parts by weight:

[0022] 22 to 30 parts of magnesium aluminum alloy powder, 7 to 13 parts of modified carbon powder, 9 to 15 parts of composite metal powder, and 1 to 7 parts of additives;

[0023] The composite metal powder is composed of Ni, Pb, Re, Cr and Be in a mass ratio of (1-3): (2-7): (1-7): (1-3): (1-2).

[0024] In one of the embodiments, it is characterized in that the auxiliary agent is at least one of cerium dioxide, boron carbide and silicon nitride.

[0025] In addition, the present application also provides a method for preparing an oxidation-resistant aluminum alloy additive, the preparation method comprising the following steps:

[0026] Add the carbon powder to ethanol, stir for 1 h to 2 h, let stand for 10 min to 25 min, filter, wash the filter cake repeatedly with water, and dry to obtain modified carbon powder;

[0027] Magnesium-aluminum metal powder, composite metal powder and additives are added to a mixing kettle for the first smelting treatment, and then modified carbon powder is added for a second smelting treatment. The jet passes through the nozzle component and meets the atomizing medium, and is dispersed into metal droplets under the action of the atomizing medium. The component powder is cooled and solidified to obtain an antioxidant aluminum alloy additive.

[0028] In one of the embodiments, the solid-liquid ratio of the carbon powder to ethanol is 1 g / (15-20) mL.

[0029] In one embodiment, the stirring temperature is 65°C to 85°C.

[0030] In one embodiment, the drying process is carried out at a temperature of 65° C. to 95° C. and for a time of 20 min to 60 min.

[0031] In one embodiment, the temperature of the first smelting treatment is 900° C. to 1500° C., the vacuum degree is 25 Pa to 35 Pa, and the time is 35 min to 55 min.

[0032] In one embodiment, the temperature of the second smelting treatment is 1200° C. to 1250° C., the atomization pressure is 0.5 MPa to 1.0 MPa, and the time is 20 min to 35 min.

[0033] In one of the embodiments, after the second smelting treatment, ultrasonic treatment is required for 10 minutes to 20 minutes, and the power of the ultrasonic treatment is 100W to 150W.

[0034] In one embodiment, the flow rate of the jet is 1 L / min to 3 L / min.

[0035] In one of the embodiments, the average particle size of the anti-oxidation aluminum alloy additive is 50 μm to 120 μm.

[0036] In one of the embodiments, the antioxidant aluminum alloy additive is applied in the preparation process of aluminum alloy.

[0037] In one of the embodiments, the amount of the antioxidant aluminum alloy additive added in the aluminum alloy preparation process accounts for 1% to 20% of the total mass of the aluminum alloy.

[0038] In the above scheme, after the magnesium-aluminum alloy powder, modified carbon powder, composite metal powder and additives are compounded, the specific components interact with each other, which has a significant promoting effect on the overall antioxidant effect.

[0039] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0040] Embodiment 1~3:

[0041] The difference between Examples 1 to 3 is that the raw materials for preparing the antioxidant aluminum alloy additive are different, and the others are the same, as shown in Table 1;

[0042] A method for preparing an oxidation-resistant aluminum alloy additive comprises the following steps:

[0043] Add carbon powder to ethanol at a concentration of 1 g / 20 mL, heat to 65°C and stir for 2 h, let stand for 20 min, filter, wash the filter cake repeatedly with water, and dry at 95°C to obtain modified carbon powder;

[0044] Magnesium-aluminum metal powder, composite metal powder and additives are added to a mixing kettle, and the first smelting treatment is carried out at a temperature of 1200°C and a vacuum of 25Pa for 35 minutes. Then, modified carbon powder is added, and a second smelting treatment is carried out at a temperature of 1250°C and an atomization pressure of 0.5MPa for 20 minutes. After the second smelting treatment, it is necessary to apply an ultrasonic action of 100W for 10 minutes, and then a jet with a flow rate of 2L / min is ejected through a nozzle component to meet the atomizing medium, and is dispersed into metal droplets under the action of the atomizing medium, and the component powder is cooled and solidified to obtain an antioxidant aluminum alloy additive with an average particle size of 50μm.

[0045] Comparative Example 10:

[0046] The difference between Comparative Example 10 and Example 3 is that the carbon powder in Comparative Example 10 is not modified, and the rest is the same as Example 3.

[0047] Comparative Example 11:

[0048] The difference between Comparative Example 11 and Example 3 is that the preparation method in Comparative Example 11 is as follows, and the preparation raw materials are the same as those in Example 3.

[0049] A method for preparing an oxidation-resistant aluminum alloy additive comprises the following steps:

[0050] Add carbon powder to ethanol at a concentration of 1 g / 20 mL, heat to 65°C and stir for 2 h, let stand for 20 min, filter, wash the filter cake repeatedly with water, and dry at 95°C to obtain modified carbon powder;

[0051] Magnesium-aluminum metal powder, composite metal powder and additives are added to a mixing kettle, smelted at a temperature of 1200°C and a vacuum of 25Pa for 55 minutes, and then a jet with a flow rate of 2L / min is ejected through a nozzle component to meet the atomizing medium and, under the action of the atomizing medium, is dispersed into metal droplets, and the component powder is cooled and solidified to obtain an antioxidant aluminum alloy additive with an average particle size of 50μm.

[0052] Table 1: Preparation of raw materials

[0053]

[0054]

[0055] The antioxidant aluminum alloy additives prepared in Examples 1 to 3 and the antioxidant aluminum alloy additives prepared in Comparative Examples 1 to 11 were respectively applied to the preparation process of the same aluminum alloy (since the present application does not require protection of the aluminum alloy material, its composition and specific process are not described in detail). In each group of tests, the amount of the antioxidant aluminum alloy additive added accounted for 10% of the total mass of the aluminum alloy. The obtained aluminum alloys were subjected to relevant performance tests, and a blank control group without the addition of the antioxidant aluminum alloy additive was set. The results are shown in Table 2 below.

[0056] Table 2: Performance test results

[0057]

[0058]

[0059] From the data analysis of Table 2, it can be seen that the present application helps to improve the corrosion resistance of aluminum alloys by optimizing the preparation of raw materials, and the addition of anti-oxidation aluminum alloy additives can promote the grain size to be smaller, and the surface has no color spots after oxidation, which can significantly improve the corrosion resistance and oxidation resistance of aluminum alloys, making them suitable for more complex use environments.

[0060] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0061] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An antioxidant aluminum alloy additive, characterized in that: The antioxidant aluminum alloy additive comprises the following raw materials in parts by weight: 22 to 30 parts of magnesium aluminum alloy powder, 7 to 13 parts of modified carbon powder, 9 to 15 parts of composite metal powder, and 1 to 7 parts of additives; The composite metal powder is composed of Ni, Pb, Re, Cr and Be in a mass ratio of (1-3): (2-7): (1-7): (1-3): (1-2).

2. The antioxidant aluminum alloy additive according to claim 1, characterized in that: The auxiliary agent is at least one of cerium dioxide, boron carbide and silicon nitride.

3. A method for preparing an antioxidant aluminum alloy additive, characterized in that: The preparation method is used to prepare the antioxidant aluminum alloy additive according to claim 1 or 2, and the preparation method comprises the following steps: Add the carbon powder to ethanol, stir for 1 h to 2 h, let stand for 10 min to 25 min, filter, wash the filter cake repeatedly with water, and dry to obtain modified carbon powder; Magnesium-aluminum metal powder, composite metal powder and additives are added to a mixing kettle for the first smelting treatment, and then modified carbon powder is added for a second smelting treatment. The jet passes through the nozzle component and meets the atomizing medium, and is dispersed into metal droplets under the action of the atomizing medium. The component powder is cooled and solidified to obtain an antioxidant aluminum alloy additive.

4. The preparation method according to claim 3, characterized in that: The solid-liquid ratio of the carbon powder to ethanol is 1 g / (15-20) mL.

5. The preparation method according to claim 3, characterized in that: The drying process is performed at a temperature of 65° C. to 95° C. and for a time of 20 min to 60 min.

6. The preparation method according to claim 3, characterized in that: The temperature of the first smelting treatment is 900° C. to 1500° C., the vacuum degree is 25 Pa to 35 Pa, and the time is 35 min to 55 min.

7. The preparation method according to claim 3, characterized in that: The temperature of the second smelting treatment is 1200° C. to 1250° C., the atomization pressure is 0.5 MPa to 1.0 MPa, and the time is 20 min to 35 min.

8. The preparation method according to claim 7, characterized in that: After the second smelting treatment, ultrasonic treatment is required for 10 to 20 minutes, and the power of the ultrasonic treatment is 100W to 150W.

9. The preparation method according to claim 3, characterized in that: The flow rate of the jet is 1 L / min to 3 L / min.

10. The preparation method according to claim 3, characterized in that: The average particle size of the anti-oxidation aluminum alloy additive is 50 μm to 120 μm.