Beta-phase high-strength Zr-series high-entropy alloy wire as well as preparation method and application thereof
By designing high-strength Zr-based high-entropy alloy wires with β phase and employing strict control of element ratios and cold rolling processes, the problem of insufficient strength and plasticity in traditional Zr-based alloys has been solved, achieving simplified preparation of high-strength, high-plasticity alloy wires suitable for the aerospace field.
Patent Information
- Application Number
- CN202411153670.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional α-phase Zr alloys have insufficient strength and limited plastic deformation capacity, making it difficult to achieve large plastic deformation through a single cold deformation process. Furthermore, the preparation process is lengthy and complex, failing to meet increasingly demanding service performance requirements.
The design of high-strength Zr-based high-entropy alloy wire with β phase involves strictly controlling the proportions of Zr, Ti, and Nb elements and adding an appropriate amount of Al to ensure a single β phase structure. The process of cold rolling and cold roll forming, combined with final annealing, achieves high strength and good cold deformation capability.
High-strength, high-plasticity, and uniform-diameter alloy wires were produced, simplifying the production process, reducing energy consumption, improving forming efficiency, and meeting the performance requirements of aerospace and other fields.
Smart Images

Figure CN118932203A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials and preparation thereof, and in particular relates to a β-phase high-strength Zr-based high-entropy alloy wire material and a preparation method and application thereof. Background Art
[0002] High-strength and tough alloy wires are widely used in aircraft carrier arresting cables, aerospace and deep space exploration key equipment. With the continuous breakthroughs in high-precision and cutting-edge technologies, the working environment of alloy wires has become increasingly harsh, and higher requirements have been placed on the limits of their service performance. Among them, Zr-based alloys and their wires are one of the most commonly used engineering materials in the fields of aerospace technology, nuclear industry, and medicine. It should be pointed out that the design of traditional α-phase Zr-based alloys only improves its mechanical properties by adding trace elements. There are generally shortcomings such as insufficient strength and limited plastic deformation capacity. The limit performance that can be explored gradually tends to a bottleneck, and there is limited room for improvement, making it difficult to meet the growing performance requirements. In addition, the deformation mechanism of traditional α-phase Zr alloys is single, and it is difficult to achieve large plastic deformation through a single cold deformation process. It needs to be supplemented by multiple stress relief or recrystallization annealing to finally achieve the preparation of alloy wires. The process is lengthy and complicated, time-consuming and labor-intensive. Summary of the invention
[0003] High entropy alloys are a type of new material developed based on "chemical disorder" at the atomic scale. They usually contain 3 or more dominant elements. They have been proven to have many excellent properties that are superior to traditional alloys, such as high strength, good strength-toughness matching, good corrosion resistance and radiation resistance. They show great development potential in the fields of aerospace, electronics, energy, etc. High entropy alloys are rich in constituent elements and have the conditions to induce a variety of coupled strengthening and toughening mechanisms. They can achieve the simultaneous improvement of strength-plasticity and have the potential to break through the performance limits of traditional alloys. They are a new type of superior candidate structural materials. In order to solve the problem that the traditional α-phase Zr-based alloys have poor cold deformation ability and difficult to break through the mechanical service performance, the present invention is based on the design concept of high entropy alloys. By regulating the composition phase stability of the alloy through the content of constituent elements, a new type of β-phase high-strength Zr-based alloy wire with high strength and good cold working deformation ability is designed and developed. On the one hand, the present invention is committed to improving the performance limit of Zr-based alloy wires, and on the other hand, improving the deformation processing ability of Zr-based alloys, especially strengthening its cold deformation processing ability, improving wire forming efficiency, and reducing production costs, which is of great significance for industrial applications.
[0004] The present invention provides a β-phase high-strength Zr-based high-entropy alloy wire and its preparation method and application. The β-phase high-strength Zr-based high-entropy alloy wire of the present invention further strictly controls the Al element content on the basis of strictly controlling the ratio of Zr, Ti and Nb elements, and strengthens the mechanical properties on the basis of ensuring that the solidified structure is a single β-phase, so as to obtain a high-strength alloy wire; at the same time, the single solid solution phase structure can ensure the implementation of the whole "cold rolling + cold rolling" cold processing preparation process, and the prepared alloy wire only needs the final finished product annealing treatment, and the wire diameter is uniform, the surface has no continuous defects, and the internal structure is uniform. Finally, the short process, low energy consumption and high-quality preparation of high-strength high-entropy alloy wire is achieved.
[0005] The present invention specifically includes the following contents:
[0006] A method for preparing a β-phase high-strength Zr-based high-entropy alloy wire comprises the following steps:
[0007] (1) Ingredients: Ingredients are prepared according to the atomic ratio of Zr 65 at.%, Ti 20 at.%, and Nb 15 at.%, and Al accounting for x at.% of the total atomic weight is added, where 0<x<10, to obtain an alloy raw material; and then the alloy raw material is washed and dried;
[0008] (2) Melting and ingot casting: Melting the dried raw materials and then casting to obtain alloy ingots;
[0009] (3) Turning and milling: cutting the alloy ingot into long strips of alloy bars, and then performing milling on the alloy bars;
[0010] (4) Cold rolling: The alloy strip after the milling treatment is subjected to profile cold rolling, and the initial deformation is controlled to be less than 10%, and the subsequent reduction in each pass is 10-20%, and the reduction in each pass is gradually reduced, and finally a rolled wire with a diameter of less than 1.5 mm is obtained by rolling;
[0011] (5) Finishing rolling of finished products: The rolled wire is subjected to finishing rolling of finished products, and the finishing rolling passes are controlled to be 1 to 3 times, and the deformation of each pass is less than 5%, so as to finally obtain a finished wire with good diameter consistency, that is, an alloy cold rolled wire, wherein the diameter of the finished wire is 0.5-1.5 mm, the tensile strength is greater than 1867 MPa, and the plastic strain is ≥3.6%.
[0012] Optionally, the step (6) of heat treatment of the finished product is further included: the finished wire is placed in a vacuum environment at 450-700°C for 10-30 minutes. It should be noted that in order to ensure the best match between the strength and plasticity of the wire, the heat treatment temperature is set to 0.3-0.45°C in the present invention. m (T m : alloy melting point), i.e. 450-700℃, and then air-cooled or water-cooled.
[0013] It should be noted that whether the finished product of the β-phase high-strength Zr-based high-entropy alloy wire of the present invention, that is, the alloy cold-rolled wire obtained after finish rolling, is annealed can be selected according to actual needs.
[0014] Preferably, each element in the alloy raw material in step (1) is pure metal particles with a purity greater than 99.9%.
[0015] Preferably, the method for cleaning the alloy raw material in step (1) is: using an ultrasonic cleaning machine to clean it using acetone, alcohol, and deionized water as cleaning agents in sequence.
[0016] Preferably, the smelting method in step (2) is: vacuum induction melting, vacuum arc melting, and / or magnetic levitation induction melting.
[0017] Preferably, the alloy ingot in step (2) is a cylindrical or cubic ingot weighing 3-10 kg.
[0018] Preferably, the alloy bar is a square bar with a cross-sectional size less than 20 mm×20 mm, or a round rod with a cross-sectional diameter less than 20 mm.
[0019] A β-phase high-strength Zr-based high-entropy alloy wire prepared by adopting the preparation method of the β-phase high-strength Zr-based high-entropy alloy wire.
[0020] An application of the β-phase high-strength Zr-based high-entropy alloy wire in aircraft carrier arresting cables, aerospace and deep space exploration equipment.
[0021] Beneficial effects of the present invention:
[0022] (1) In order to solve the problem of poor cold deformation ability of α-phase Zr-based alloys, the present invention designs a β-phase high-strength Zr-based high-entropy alloy wire with good cold deformation ability. The β-phase high-strength Zr-based high-entropy alloy wire of the present invention strictly controls the atomic ratio of the three elements Zr, Ti, and Nb to 65:20:15, and can obtain a single β solid solution phase structure to ensure the cold deformation processing ability of the alloy. On this basis, the present invention adds Al and strictly controls the total atomic content of the Al element to be greater than 0% and less than 10%, which can play an enhancing role while ensuring the cold deformation ability of the alloy, thereby achieving the strengthening of the mechanical properties of the wire.
[0023] (2) Based on the design of the components of the alloy wire, the present invention provides a wire preparation method specifically for the alloy described in the present invention, firstly, the profile is cold rolled, the initial deformation is controlled to be less than 10%, and the subsequent reduction in each pass is 10-20%, and the reduction in each rolling pass decreases successively, and finally a rolled wire with a diameter of less than 1.5 mm is obtained by rolling; then, the rod-tied wire is subjected to finished product finish rolling, the finished product finish rolling passes are controlled to be 1 to 3 times, and the deformation in each pass is less than 5%, and finally a finished wire with good diameter consistency is obtained, and the diameter of the finished wire is 0.5-1.5 mm, the tensile strength is ≥1867 MPa, and the plastic strain is ≥3.6%. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The morphology diagram of the β-phase high-strength Zr-based high-entropy alloy wire prepared in Example 4 of the present invention, wherein (a) and (b) are macroscopic morphology diagrams, (c) is a microscopic morphology diagram under a scanning electron microscope, and (d) is an X-ray diffraction diagram of the β-phase high-strength Zr-based high-entropy alloy wire;
[0025] Figure 2 This is a tensile performance diagram of the β-phase high-strength Zr-based high-entropy alloy wire prepared in Example 4 of the present invention;
[0026] Figure 3 The microscopic morphology of the tensile specimen of the β-phase high-strength Zr-based high-entropy alloy wire prepared in Example 4 of the present invention, wherein (a) is the fracture morphology and (b) is the tensile specimen morphology. DETAILED DESCRIPTION
[0027] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments shown below do not limit the invention content described in the claims. In addition, the entire contents of the structures represented by the following embodiments are not limited to those necessary as solutions to the invention described in the claims.
[0028] A method for preparing a β-phase high-strength Zr-based high-entropy alloy wire comprises the following steps:
[0029] (1) Ingredients: Ingredients are prepared according to the atomic ratio of Zr 65 at.%, Ti 20 at.%, and Nb 15 at.%, and Al accounting for x at.% of the total atomic weight is added, wherein 0<x<10, and each element is pure metal particles with a purity greater than 99.9%, to obtain an alloy raw material; and then the alloy raw material is cleaned with acetone, alcohol, and deionized water in an ultrasonic cleaning machine in sequence, and then dried;
[0030] (2) Melting and ingot casting: The dried raw materials are subjected to vacuum induction melting, vacuum arc melting, and / or magnetic levitation induction melting, and then cast to obtain a cylindrical or cubic alloy ingot weighing 3-10 kg. If Zr, Ti, and Nb are regarded as a whole and Al is regarded as an additional element, the composition of the alloy can be expressed as Zr 65 Ti 20 Nb 15 -Al x (0<x<10, at.%); if all elements are considered as a whole, the composition of the alloy can be expressed as Zr 59-65 Ti 18-20 Nb 13.6- 15 Al x (0<x<10, at.%), that is, the total composition of the alloy is: Zr 59-65 at.%, Ti 18-20 at.%, Nb 13.6-15 at.%, 0 at.%<Al<10 at.%;
[0031] (3) Turning and milling: cutting the alloy ingot into alloy bars with a cross-sectional size of less than 20 mm×20 mm, or round alloy bars with a cross-sectional diameter of less than 20 mm, and then performing milling on the alloy bars;
[0032] (4) Cold rolling: The alloy strip after the milling treatment is subjected to profile cold rolling, and the initial deformation is controlled to be less than 10%, and the subsequent reduction in each pass is 10-20%, and the reduction in each pass is gradually reduced, and finally a rolled wire with a diameter of less than 1.5 mm is obtained by rolling;
[0033] (5) Finishing rolling of finished products: The rolled wire is subjected to finishing rolling of finished products, and the finishing rolling passes are controlled to be 1 to 3 times, and the deformation of each pass is less than 5%, so as to finally obtain a finished wire with good diameter consistency; the diameter of the finished wire is 0.5-1.5 mm, the tensile strength is ≥1867 MPa, and the plastic strain is ≥3.6%;
[0034] (6) Finished product heat treatment: The finished wire is placed in a vacuum environment at 450-700°C for 10-30 minutes, and then air-cooled or water-cooled to obtain the final β-phase high-strength Zr-based high-entropy alloy wire.
[0035] The β-phase high-strength Zr-based high-entropy alloy wire prepared by the preparation method of the β-phase high-strength Zr-based high-entropy alloy wire can be applied to aircraft carrier arresting cables, aerospace and deep space exploration equipment.
[0036] Example 1
[0037] A method for preparing a β-phase high-strength Zr-based high-entropy alloy wire comprises the following steps:
[0038] Step 1: The composition of the β-phase high-strength Zr-based high-entropy alloy wire is designed to be Zr 65 Ti 20 Nb 15 -Al3;
[0039] Step 2, select 99.9% pure metal element particles of Ti, Zr, Nb, and Al, weigh them using an electronic balance with 3 decimal places, and use an ultrasonic cleaner to clean and dry the high-purity metal raw materials in acetone, alcohol, and deionized water in turn;
[0040] Step 3, adding the cleaned raw materials into a vacuum induction melting furnace for melting, repeatedly melting for 6 times, casting into a graphite mold, and preparing a 7 kg cylindrical billet;
[0041] Step 4, the prepared alloy ingot is subjected to wire cutting processing to be cut into square strips with a cross-section of 15 mm×15 mm, and the alloy strips are subjected to milling and smoothing treatment;
[0042] Step 5, placing the obtained alloy on a profile rolling mill for cold rolling, adjusting the mold to ensure that the initial deformation is less than 10%, performing the first cold rolling, and controlling the deformation range of each subsequent rolling pass to be 10% to 20%. In this case, the wire diameter after cold rolling is in the range of 0.8 to 0.85 mm.
[0043] Step 6, perform two passes of finish rolling on the cold rolled wire, accurately control the wire diameter, and control the single deformation amount to 3% to 5%, and finally obtain an alloy wire with a diameter of 0.8mm±0.05, that is, an alloy cold rolled wire.
[0044] The alloy cold-rolled wire obtained in step 6 of this embodiment was subjected to a tensile test of mechanical properties, and the room temperature tensile strength was 1867 MPa, and the plastic strain was 4.1%.
[0045] Step 7, the obtained alloy wire is subjected to stress relief annealing, the alloy wire is vacuum annealed at 550° C., the heat preservation time is 20 minutes, and air-cooled.
[0046] Example 2
[0047] A method for preparing a β-phase high-strength Zr-based high-entropy alloy wire comprises the following steps:
[0048] Step 1: The composition of the β-phase high-strength Zr-based high-entropy alloy wire is designed to be Zr 65 Ti 20 Nb 15 -Al5;
[0049] Step 2, select 99.9% pure metal element particles of Ti, Zr, Nb, and Al, weigh them using an electronic balance with 3 decimal places, and use an ultrasonic cleaner to clean and dry the high-purity metal raw materials in acetone, alcohol, and deionized water in turn;
[0050] Step 3, adding the cleaned raw materials into a vacuum induction melting furnace for melting, repeatedly melting for 6 times, casting into a graphite mold, and preparing a 7 kg cylindrical billet;
[0051] Step 4, the prepared alloy ingot is subjected to wire cutting processing to be cut into square strips with a cross-section of 15 mm×15 mm, and the alloy strips are subjected to milling and smoothing treatment;
[0052] Step 5, placing the obtained alloy on a profile rolling mill for cold rolling, adjusting the mold to ensure that the initial deformation is less than 10%, performing the first cold rolling, and controlling the deformation range of each subsequent rolling pass to be 10% to 20%. In this case, the wire diameter after cold rolling is in the range of 0.8 to 0.85 mm.
[0053] Step 6, perform two passes of finish rolling on the cold rolled wire, accurately control the wire diameter, and control the single deformation amount to 3% to 5%, and finally obtain an alloy wire with a diameter of 0.8mm±0.05, that is, an alloy cold rolled wire.
[0054] The alloy cold-rolled wire obtained in step 6 of this embodiment was subjected to a tensile test of mechanical properties, and the room temperature tensile strength was 1873 MPa, and the plastic strain was 4.0%.
[0055] Step 7, the obtained alloy wire is subjected to stress relief annealing, the alloy wire is vacuum annealed at 500° C., the heat preservation time is 20 minutes, and air-cooled.
[0056] Example 3
[0057] A method for preparing a β-phase high-strength Zr-based high-entropy alloy wire comprises the following steps:
[0058] Step 1: The composition of the β-phase high-strength Zr-based high-entropy alloy wire is designed to be Zr 65 Ti 20 Nb 15 -Al7;
[0059] Step 2, select 99.9% pure metal element particles of Ti, Zr, Nb, and Al, weigh them using an electronic balance with 3 decimal places, and use an ultrasonic cleaner to clean and dry the high-purity metal raw materials in acetone, alcohol, and deionized water in turn;
[0060] Step 3, adding the cleaned raw materials into a vacuum induction melting furnace for melting, repeatedly melting for 6 times, casting into a graphite mold, and preparing a 7 kg cylindrical billet;
[0061] Step 4, the prepared alloy ingot is subjected to wire cutting processing to be cut into square strips with a cross-section of 15 mm×15 mm, and the alloy strips are subjected to milling and smoothing treatment;
[0062] Step 5, placing the obtained alloy on a profile rolling mill for cold rolling, adjusting the mold to ensure that the initial deformation is less than 10%, performing the first cold rolling, and controlling the deformation range of each subsequent rolling pass to be 10% to 20%. In this case, the wire diameter after cold rolling is in the range of 1 to 1.15 mm.
[0063] Step 6, perform two passes of finish rolling on the cold rolled wire, accurately control the wire diameter, and control the single deformation amount to 3% to 5%, and finally obtain an alloy wire with a diameter of 1mm±0.05, that is, an alloy cold rolled wire.
[0064] The alloy cold-rolled wire obtained in step 6 of this embodiment was subjected to a tensile test of mechanical properties, and the room temperature tensile strength was 1878 MPa, and the plastic strain was 3.9%.
[0065] Step 7, the obtained alloy wire is subjected to stress relief annealing, the alloy wire is vacuum annealed at 450° C., the heat preservation time is 20 minutes, and air-cooled.
[0066] Example 4
[0067] A method for preparing a β-phase high-strength Zr-based high-entropy alloy wire comprises the following steps:
[0068] Step 1: The composition of the β-phase high-strength Zr-based high-entropy alloy wire is designed to be Zr 65 Ti 20 Nb 15 -Al9;
[0069] Step 2, select 99.9% pure metal element particles of Ti, Zr, Nb, and Al, weigh them using an electronic balance with 3 decimal places, and use an ultrasonic cleaner to clean and dry the high-purity metal raw materials in acetone, alcohol, and deionized water in turn;
[0070] Step 3, adding the cleaned raw materials into a vacuum induction melting furnace for melting, repeatedly melting for 6 times, casting into a graphite mold, and preparing a 7 kg cylindrical billet;
[0071] Step 4, the prepared alloy ingot is subjected to wire cutting processing to be cut into square strips with a cross-section of 15 mm×15 mm, and the alloy strips are subjected to milling and smoothing treatment;
[0072] Step 5, placing the obtained alloy on a profile rolling mill for cold rolling, adjusting the mold to ensure that the initial deformation is less than 10%, performing the first cold rolling, and controlling the deformation range of each subsequent rolling pass to be 10% to 20%. In this case, the wire diameter after cold rolling is in the range of 1.5 to 1.65 mm.
[0073] Step 6, perform two passes of finish rolling on the cold rolled wire, accurately control the wire diameter, and control the single deformation amount to 3% to 5%, and finally obtain an alloy wire with a diameter of 1.5mm±0.05, that is, an alloy cold rolled wire.
[0074] The alloy cold rolled wire prepared in step 6 of Example 4 was observed and tested. Figure 1 The morphology of the β-phase high-strength Zr-based high-entropy alloy wire prepared in Example 4, wherein (a) and (b) are macroscopic morphology images, and it can be observed that the wire has good forming performance; (c) is a microscopic morphology image under a scanning electron microscope, and the surface quality of the wire is good, there are no macro cracks, and the finish is good; (d) is an X-ray diffraction image of the β-phase high-strength Zr-based high-entropy alloy wire, indicating that the alloy has a single-phase body-centered cubic structure; Figure 2 This is a tensile performance diagram of the β-phase high-strength Zr-based high-entropy alloy wire prepared in Example 4 of the present invention; Figure 3 The microscopic morphology of the tensile specimen of the β-phase high-strength Zr-based high-entropy alloy wire prepared in Example 4 of the present invention, where (a) is the fracture morphology and (b) is the tensile specimen morphology. The fracture morphology shows typical ductile fracture characteristics, and the fracture is covered with dense dimples, indicating that the alloy wire has good tensile mechanical properties.
[0075] The alloy cold rolled wire obtained in step 6 of Example 4 was subjected to a tensile test of mechanical properties, and the room temperature tensile strength was 1875 MPa, and the plastic strain was 3.6%.
[0076] The cold rolled alloy wire obtained in step 6 of Example 4 was annealed at 550°C for 25 minutes and then air-cooled, and its room temperature tensile strength was 1453 MPa and the plastic strain was 7.6%. This is mainly attributed to the fact that after annealing, the internal dislocation density of the alloy wire was reduced, and the grains recovered and grew during the annealing and air-cooling process, which increased the plastic deformation ability of the alloy and reduced the strength.
[0077] The cold rolled alloy wire obtained in step 6 of Example 4 was annealed at 550°C for 25 minutes and then water-cooled. The room temperature tensile strength was 1611 MPa and the plastic strain was 5.4%. This is mainly due to the fact that after annealing, the internal dislocation density of the alloy wire decreased, and the grains recovered and grew during the annealing process, which improved the plastic deformation ability of the alloy and reduced the strength. Compared with air cooling, the water cooling method limits the growth of the grains during the cooling process, making its plasticity between the wire without heat treatment and the air-cooled wire.
[0078] Comparative Example 1
[0079] Step 1: The composition of the β-phase high-strength Zr-based high-entropy alloy wire is designed to be Zr 65 Ti 20 Nb 15 -Al9;
[0080] Step 2, select 99.9% pure metal element particles of Ti, Zr, Nb, and Al, weigh them using an electronic balance with 3 decimal places, and use an ultrasonic cleaner to clean and dry the high-purity metal raw materials in acetone, alcohol, and deionized water in turn;
[0081] Step 3, adding the cleaned raw materials into a vacuum induction melting furnace for melting, repeatedly melting for 6 times, casting into a graphite mold, and preparing a 7 kg cylindrical billet;
[0082] Step 4, the prepared alloy ingot is subjected to wire cutting processing to be cut into square strips with a cross-section of 15 mm×15 mm, and the alloy strips are subjected to milling and smoothing treatment;
[0083] Step 5: placing the obtained alloy on a profile rolling mill for hot rolling at a temperature of 650° C. The die is adjusted to ensure that the initial deformation is less than 10%.
[0084] The alloy composition of this comparative example is consistent with that of Example 4, and the cold rolling process is converted into a hot rolling process. As a result, the alloy rods are brittlely fractured during the preparation process, and the alloy wires cannot be rolled by hot rolling.
[0085] Comparative Example 2
[0086] Step 1: The composition of the β-phase high-strength Zr-based high-entropy alloy wire is designed to be Zr 65 Ti 20 Nb 15 -Al 20 ;
[0087] Step 2, select 99.9% pure metal element particles of Ti, Zr, Nb, and Al, weigh them using an electronic balance with 3 decimal places, and use an ultrasonic cleaner to clean and dry the high-purity metal raw materials in acetone, alcohol, and deionized water in turn;
[0088] Step 3, adding the cleaned raw materials into a vacuum induction melting furnace for melting, repeatedly melting for 6 times, casting into a graphite mold, and preparing a 7 kg cylindrical billet;
[0089] Step 4, the prepared alloy ingot is subjected to wire cutting processing to be cut into square strips with a cross-section of 15 mm×15 mm, and the alloy strips are subjected to milling and smoothing treatment;
[0090] Step 5, placing the obtained alloy on a profile rolling mill for cold rolling, adjusting the mold to ensure that the initial deformation is less than 10%, performing the initial cold rolling, and controlling the deformation range of each subsequent rolling pass to be 10% to 20%.
[0091] The process of this comparative example is consistent with that of Example 4, but the alloy composition is different (different Al content). The results show that when the alloy deformation is ~60%, the alloy bar breaks brittlely, and the bar diameter is 9.5mm×9.5mm, and cold rolling cannot be continued.
[0092] A comparison of the alloys, processing methods and technical effects of Examples 1-4 of the present invention and Comparative Examples 1-2 is shown in Table 1. It can be seen from Table 1 that only when the conditions of the alloy composition of the present invention and the cold rolling process are met can a qualified β-phase high-strength Zr-based high-entropy alloy wire be prepared.
[0093] Table 1 Comparison of alloys, processing methods and technical effects of the embodiments of the present invention and the comparative examples
[0094] Case Category Alloy composition Molding process Effect Example 1 <h2 style=";text-align:left;direction:ltr"><![CDATA[Zr <h2 style=";text-align:left;direction:ltr"> 65 <h2 style=";text-align:left;direction:ltr"> Ti<h2 style=";text-align:left;direction:ltr"> 20 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 15 <h2 style=";text-align:left;direction:ltr"> -Al3]]><h2 style=";text-align:left;direction:ltr"> Multi-pass cold rolling Good formability Example 2 <![CDATA[Zr 65 Of 20 Nb 15 -Al5]]> Multi-pass cold rolling Good formability Example 3 <h2 style=";text-align:left;direction:ltr"><![CDATA[Zr <h2 style=";text-align:left;direction:ltr"> 65 <h2 style=";text-align:left;direction:ltr"> Ti<h2 style=";text-align:left;direction:ltr"> 20 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 15 <h2 style=";text-align:left;direction:ltr"> -Al7]]><h2 style=";text-align:left;direction:ltr"> Multi-pass cold rolling Good formability Example 4 <![CDATA[Zr 65 The 20 Nb 15 -Al9]]> Multi-pass cold rolling Good formability Comparative Example 1 <![CDATA[Zr 65 The 20 Nb 15 -Al9]]> Multi-pass hot rolling Hot rolling cannot be carried out, and alloy bars are cracked Comparative Example 2 <![CDATA[Zr 65 The 20 Nb 15 -Al 20 ]]> Multi-pass cold rolling The plastic deformation capacity is limited, and the alloy bar is rolled and cracked.
[0095] In summary, the β-phase high-strength Zr-based high-entropy alloy wire of the present invention has good comprehensive mechanical properties and cold working formability, the preparation method is safe and reliable, simple and easy, and has the advantages of low energy consumption and short process, and has broad industrial application prospects. The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention are covered within the protection scope of the present invention.
[0096] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a β-phase high-strength Zr-based high-entropy alloy wire, characterized in that: The following steps are involved: (1) Ingredients: Ingredients are prepared according to the atomic ratio of Zr 65 at.%, Ti 20 at.%, and Nb 15 at.%, and Al accounting for x at.% of the total atomic weight is added, where 0<x<10, to obtain an alloy raw material; and then the alloy raw material is washed and dried; (2) Melting and ingot casting: Melting the dried raw materials and then casting to obtain alloy ingots; (3) Turning and milling: cutting the alloy ingot into long strips of alloy bars, and then performing milling on the alloy bars; (4) Cold rolling: The alloy strip after the milling treatment is subjected to profile cold rolling, and the initial deformation is controlled to be less than 10%, and the subsequent reduction in each pass is 10-20%, and the reduction in each pass is gradually reduced, and finally a rolled wire with a diameter of less than 1.5 mm is obtained by rolling; (5) Finishing rolling of finished products: The rolled wire is subjected to finishing rolling of finished products, and the finishing rolling passes are controlled to be 1 to 3 times, and the deformation of each pass is less than 5%, so as to finally obtain a finished wire with good diameter consistency. The diameter of the finished wire is 0.5-1.5 mm, the tensile strength is ≥1867 MPa, and the plastic strain is ≥3.6%.
2. The method for preparing a β-phase high-strength Zr-based high-entropy alloy wire according to claim 1, characterized in that: The method further comprises step (6) heat treatment of the finished product: placing the finished wire material in a vacuum environment at 450-700° C. for 10-30 minutes, and then air cooling or water cooling.
3. The method for preparing a β-phase high-strength Zr-based high-entropy alloy wire according to claim 1, characterized in that: All elements in the alloy raw material of step (1) are pure metal particles with a purity greater than 99.9%.
4. The method for preparing a β-phase high-strength Zr-based high-entropy alloy wire according to claim 1, characterized in that: The cleaning method of the alloy raw material in step (1) is: using an ultrasonic cleaning machine to clean it using acetone, alcohol and deionized water as cleaning agents in sequence.
5. The method for preparing a β-phase high-strength Zr-based high-entropy alloy wire according to claim 1, characterized in that: The smelting method in step (2) is: vacuum induction melting, vacuum arc melting, and / or magnetic levitation induction melting.
6. The method for preparing a β-phase high-strength Zr-based high-entropy alloy wire according to claim 1, characterized in that: The alloy ingot in step (2) is a cylindrical or cubic ingot weighing 3-10 kg.
7. The method for preparing a β-phase high-strength Zr-based high-entropy alloy wire according to any one of claims 1 to 6, characterized in that: The alloy bar is a square bar with a cross-sectional size less than 20 mm×20 mm, or a round rod with a cross-sectional diameter less than 20 mm.
8. A β-phase high-strength Zr-based high-entropy alloy wire prepared by the method for preparing a β-phase high-strength Zr-based high-entropy alloy wire according to any one of claims 1 to 7.
9. Application of the β-phase high-strength Zr-based high-entropy alloy wire according to claim 8 in aircraft carrier arresting cables, aerospace and deep space exploration equipment.