Zinc alloy plate strip and preparation method and application thereof

By adding specific components to zinc alloy sheets and adopting continuous casting method and cold rolling preparation process, the problems of poor forming effect and low production efficiency of zinc alloy sheets are solved, and high forming performance and surface quality are improved.

CN118932215APending Publication Date: 2024-11-12CHINALCO MATERIALS APPL RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411034255.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing zinc alloy sheet preparation methods, there are problems such as poor forming effect, unstable surface quality and low production efficiency, especially defects caused by insufficient cooling strength of aluminum alloy sheets and poor quality of ingots.

Method used

The optimized zinc alloy plate and strip composition and preparation method include adding Al, Cu, Ti and rare earth elements to the zinc alloy, improving melt purity through powder refining and online filtration, and using continuous casting to improve the The casting billet was prepared at a cooling rate, followed by cold rolling to prepare the strip.

Benefits of technology

The forming performance and surface quality of zinc alloy sheet strips have been significantly improved, the looseness and pore defects inside the casting billet have been eliminated, the production efficiency and yield have been improved, and the demand for high forming performance has been met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932215A_ABST
    Figure CN118932215A_ABST
Patent Text Reader

Abstract

The invention provides a zinc alloy plate strip and a preparation method and application thereof. The preparation method comprises the following steps: S1, mixing and smelting raw materials according to the composition of the zinc alloy plate strip to obtain a liquid zinc alloy melt, and carrying out in-furnace treatment and online treatment on the liquid zinc alloy melt to obtain a purified zinc alloy melt; s2, the purified zinc alloy melt is cast through a continuous casting method, the casting temperature ranges from 400 DEG C to 440 DEG C, and a zinc alloy casting blank is prepared; and S3, the casting blank is subjected to cold rolling, and the zinc alloy plate strip is obtained. By optimizing the composition of the zinc alloy plate strip and combining a proper preparation process, the prepared zinc alloy plate strip is uniform and fine in structure, and the forming performance of the plate strip is greatly improved. The zinc alloy casting blank is prepared through a continuous casting method, the cooling strength in the casting process is high, and the production efficiency of the casting blank is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of zinc alloy material manufacturing, and in particular to a zinc alloy plate and strip material, and a preparation method and application thereof. Background Art

[0002] In recent years, with the development of the national economy, zinc alloys have been widely used in many fields such as automobiles, construction, household hardware and lamps due to their excellent properties such as low melting point, good casting performance, corrosion resistance and easy forming.

[0003] The use of zinc alloy sheets as building facades does not require anodizing treatment. It has many advantages such as good forming performance, self-cleaning, low cost and long service life. It is one of the important application areas in the future.

[0004] The conventional method for preparing zinc alloy sheets is to prepare ingot blanks by metal mold gravity casting, obtain ingot blanks of a certain size through machining and other methods, and then roll them into sheets. At present, the use of metal mold gravity casting to prepare zinc alloy ingots generally has prominent problems such as a large number of loose, shrinkage holes and even cracks inside the ingots. Under the traditional casting method, the quality of the ingot is adversely affected by the low and uneven cooling intensity, and the sheet is prone to breakage or even cracking due to ingot defects during the rolling process, which deteriorates the mechanical properties of the sheet and reduces the yield rate.

[0005] At present, the aluminum alloy plates that are widely used in the construction field have a high degree of alloying, coarse compounds, large fluctuations in forming performance, and unstable surface quality. It is urgent to develop higher performance plates to solve existing problems. Summary of the invention

[0006] The main purpose of the present invention is to provide a zinc alloy sheet and strip, a preparation method and application thereof, so as to solve the problems in the prior art that the forming effect of aluminum alloy sheets or strips is poor and the surface quality is unstable.

[0007] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing a zinc alloy sheet and strip is provided. The zinc alloy sheet and strip is composed of the following components by mass percentage: Al is 0.5% to 5%, Cu is 0.05% to 0.3%, Ti is 0.05% to 0.2%, Mn≤0.01%, one or more of the rare earth elements La, Ce, Sc and Er, the content of each rare earth element is 0.01% to 0.3%, and the balance is Zn and inevitable impurities. The preparation method comprises: step S1, mixing and smelting raw materials according to the composition of the zinc alloy sheet and strip to obtain a liquid zinc alloy melt, and subjecting the liquid zinc alloy melt to furnace treatment and online treatment to obtain a purified zinc alloy melt; step S2, casting the purified zinc alloy melt by a continuous casting method at a casting temperature of 400 to 440°C to prepare a zinc alloy ingot; step S3, cold rolling the ingot to obtain a zinc alloy sheet and strip.

[0008] Furthermore, the zinc alloy sheet and strip is composed of the following components, measured by mass percentage: Al is 0.75% to 4.65%, Cu is 0.1% to 0.27%, Ti is 0.06% to 0.18%, Mn≤0.01%, one or more of the rare earth elements La, Ce, Sc and Er, the content of each rare earth element is 0.01% to 0.25%, and the balance is Zn and unavoidable impurities.

[0009] Furthermore, in step S1, the smelting temperature is 460-520°C.

[0010] Further, the in-furnace treatment includes refining by blowing a refining agent into the melt through a high-purity inert gas using a powder spray refining method;

[0011] The refining temperature is 450-490°C and the refining time is 15-30 minutes;

[0012] Preferably, the in-furnace treatment further comprises: standing still for 15 to 25 minutes after refining.

[0013] Furthermore, the zinc alloy melt after treatment in the furnace begins to flow at 430-460°C for online treatment;

[0014] The in-line processing includes: passing the melt through an in-line filter box and a front box in sequence;

[0015] Preferably, the online filter box uses plate filtration, and the filter plate of the plate filtration has a mesh size of 40 to 60;

[0016] Preferably, the online filter box is a double-plate filter.

[0017] Further, in step S2, the casting speed is 0.5-2 m / min;

[0018] The thickness of the zinc alloy casting billet is 6 to 10 mm. Preferably, the manufacturing efficiency of the zinc alloy casting billet is ≥ 8 t / h;

[0019] The cooling rate of the casting is ≥80°C / s, preferably, the cooling rate is ≥100°C / s.

[0020] Further, in step S3, the deformation amount of the cold rolling pass is ≥40%;

[0021] Preferably, the thickness of the zinc alloy sheet strip is 0.5-1.5 mm.

[0022] According to another aspect of the present invention, a zinc alloy sheet and strip is provided. The zinc alloy sheet and strip is prepared by any one of the above-mentioned preparation methods.

[0023] Furthermore, the average grain size of the zinc alloy sheet and strip is ≤15 μm, the tensile strength is ≥160 MPa, the yield strength is ≥100 MPa, the elongation is ≥85%, and the cupping value is ≥10 mm.

[0024] According to another aspect of the present invention, there is provided a use of any one of the above-mentioned zinc alloy sheet strips as a building facade.

[0025] By applying the technical solution of the present invention, by optimizing the composition of zinc alloy sheet and strip, and combining with a suitable preparation process, the prepared zinc alloy sheet and strip has a uniform and fine structure, which greatly improves the forming performance of the sheet and strip, and solves the problem of unstable surface quality and forming performance of the current aluminum alloy sheet or strip. Among them, by regulating the smelting and melt treatment process, the purity of the melt is improved, the defects such as looseness and pores inside the ingot are eliminated, and the metallurgical quality of the ingot is guaranteed; further, in view of the prominent problem of low production efficiency caused by insufficient cooling intensity in the current preparation of zinc alloy ingots by metal mold gravity casting, the present invention adopts a continuous casting method to prepare zinc alloy ingots, and the cooling intensity of the casting process is high, which improves the production efficiency of the ingot. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0027] Figure 1 A metallographic photograph of a finished zinc alloy sheet according to Example 1 of the present invention is shown;

[0028] Figure 2 A coating photograph of a finished zinc alloy sheet material according to Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0029] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0030] As analyzed in the background technology of this application, the prior art has the problem that the aluminum alloy sheet or strip has poor forming effect and unstable surface quality. In order to solve this problem, this application provides a zinc alloy sheet or strip, a preparation method and application thereof.

[0031] According to a typical embodiment of the present application, a method for preparing a zinc alloy sheet and strip is provided, wherein the zinc alloy sheet and strip is composed of the following components, measured by mass percentage: Al is 0.5% to 5%, Cu is 0.05% to 0.3%, Ti is 0.05% to 0.2%, Mn≤0.01%, one or more of the rare earth elements La, Ce, Sc and Er, the content of each rare earth element is 0.01% to 0.3%, and the balance is Zn and unavoidable impurities. The preparation method comprises: step S1, mixing and smelting raw materials according to the composition of the zinc alloy sheet and strip to obtain a liquid zinc alloy melt, and subjecting the liquid zinc alloy melt to in-furnace treatment and online treatment to obtain a purified zinc alloy melt; step S2, casting the purified zinc alloy melt by a continuous casting method, the casting temperature is 400 to 440°C, and a zinc alloy ingot is prepared; step S3, rolling the ingot to obtain a zinc alloy sheet and strip.

[0032] This application optimizes the composition of zinc alloy sheet and strip, combines with appropriate preparation process, makes the prepared zinc alloy sheet and strip uniform and fine, greatly improves the forming performance of sheet and strip, and solves the problem of unstable surface quality and forming performance of current aluminum alloy sheet or strip. Among them, by regulating the smelting and melt treatment process, the purity of the melt is improved, the defects such as looseness and pores inside the ingot are eliminated, and the metallurgical quality of the ingot is guaranteed; further, in view of the outstanding problem of low production efficiency caused by insufficient cooling intensity in the current preparation of zinc alloy ingots by metal mold gravity casting, the present invention adopts continuous casting method to prepare zinc alloy ingots, the cooling intensity of the casting process is high, and the production efficiency of the ingot is improved.

[0033] In the preparation method of the present application, copper is added to the zinc alloy sheet and strip. The Cu element mainly forms the ε phase except that it is partially dissolved in α-Al and η-Zn. Cu inhibits the metastable β phase transformation, improves the strength, hardness and corrosion resistance of the alloy, and improves the fluidity and wear resistance of the alloy. However, excessive addition will reduce the impact toughness and dimensional stability of the zinc alloy. The copper content is controlled within the range of 0.05% to 0.35wt%, which can give full play to its role in improving the strength, hardness and corrosion resistance of the zinc alloy without affecting the impact toughness and dimensional stability of the zinc alloy. As an example, the copper content in the zinc alloy sheet and strip is 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3% or 0.35% by mass, but is not limited to this.

[0034] In zinc alloys, Al elements mainly form primary α dendrites and eutectic α phases in the form of α-Al solid solution. A small amount of Al is dissolved in η-Zn solid solution, which can refine the grains, thereby improving the strength of zinc alloys, improving alloy fluidity, reducing the oxidation tendency of alloys, improving the strength and impact toughness of zinc alloys, and reducing the corrosion of molten zinc to iron containers; however, excessive aluminum content will have an adverse effect on the strength of zinc alloys. The Al content in the zinc alloy sheet and strip of the present application is 0.5% to 5%, which is better for improving the performance of the alloy. Exemplarily, by mass percentage, the Al content can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, but is not limited thereto.

[0035] Regarding the addition of Ti, the Ti element is in the form of Al-Ti-B wire rods, and it reacts with Al to form Al3Ti through peritectic reaction, which can play a role in refining grains, especially when its content is 0.05% to 0.2%. As an example, the titanium content in the zinc alloy sheet and strip is 0.05%, 0.08%, 0.1%, 0.12%, 0.15%, 0.18% or 0.2% by mass, but it is not limited thereto.

[0036] Furthermore, adding rare earth elements La, Ce, Sc or Er to the zinc alloy sheet and strip can not only refine the grains, but also discontinuous the ε phase and refine the α phase, thereby improving the comprehensive mechanical properties of the alloy. In order to better play the role of rare earth elements and reduce the preparation cost of zinc alloy sheet and strip, the content of each rare earth element does not exceed 0.3%.

[0037] The components in the zinc alloy sheet and strip of the present application cooperate with each other, and combined with the preparation process of the present application, it has good surface quality and forming performance.

[0038] It should be noted that the present application adopts a continuous casting method for casting, and the cooling intensity of the casting process is high, which improves the production efficiency of the ingot and solves the outstanding problem of low production efficiency caused by insufficient cooling intensity in the current preparation of zinc alloy ingots by metal mold gravity casting. And the casting temperature is limited to 400-440°C. At this temperature, the fluidity of the alloy melt is good, which is conducive to reducing the internal stress and grain refinement of the casting, improving the strength and toughness of the casting, and easily obtaining a casting with a smooth surface and no defects; if the casting temperature is too high, the zinc alloy is prone to oxidation, deterioration, burning and other problems, affecting the surface quality and dimensional accuracy of the casting; if the temperature is too low, the metal liquid may not be fully filled during the filling process, resulting in internal defects and pores in the casting. In addition, too low a casting temperature is also prone to cause the metal solidification rate to be too fast, the grains are too large, and the mechanical properties of the casting are affected. Illustratively, the casting temperature is 400° C., 405° C., 410° C., 415° C., 420° C., 425° C., 430° C., 435° C., or 440° C., but is not limited thereto.

[0039] In some preferred embodiments of the present application, in order to further improve the synergistic effect between the components and to be more conducive to improving the surface quality and forming performance of the zinc alloy, the zinc alloy sheet and strip is composed of the following components by mass percentage: Al is 0.75% to 4.65%, Cu is 0.1% to 0.27%, Ti is 0.06% to 0.18%, Mn ≤ 0.01%, one or more of the rare earth elements La, Ce, Sc and Er, the content of each rare earth element is 0.01% to 0.25%, and the balance is Zn and unavoidable impurities. Preferably, the total amount of rare earth elements added is not less than 0.01wt%. Typically, but not limiting, the total amount of rare earth elements added is 0.01wt%, 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1wt%, 1.05wt%, 1.1wt%, 1.15wt%, 1.2wt% or any range therebetween.

[0040] In step S1, raw materials are mixed and smelted according to the composition of the zinc alloy sheet and strip, wherein the raw materials can be selected by technicians in the field from the prior art, and the present application has no limitation on this. For example, the raw materials include but are not limited to zinc ingots, copper-zinc alloys, zinc-titanium alloys, copper-titanium alloys, and rare earth metals.

[0041] In some embodiments of the present application, pure zinc ingots and other alloy fluxes prepared in proportion are added into a smelting furnace, heated to a temperature until they are melted into a liquid zinc alloy melt, and then uniformly mixed to obtain a liquid zinc alloy melt.

[0042] In order to better adjust the crystal structure and grain size of the melted material and further improve the surface quality and forming performance of the zinc alloy sheet and strip, in some embodiments of the present application, the melting temperature is 460-520° C. As an example, the melting temperature is 460° C., 465° C., 470° C., 475° C., 480° C., 485° C., 490° C., 495° C., 500° C., 505° C., 515° C., 510° C. or 520° C., but is not limited thereto.

[0043] In some embodiments of the present application, the above-mentioned furnace treatment includes using a powder spray refining method to blow a refining agent into the melt through a high-purity inert gas for refining, the purpose of which is to remove impurities, purify substances, enhance the performance of materials, and make the product purer, stronger, and have better surface quality. The type of refining agent can be selected from the prior art and is not particularly limited in the present application. As an example, the refining agent is one or more of hexachloroethane, zinc chloride and ammonium chloride.

[0044] In some embodiments of the present application, the refining temperature is 450-490°C and the time is 15-30 minutes, which is conducive to further improving the performance of the zinc alloy. At the above refining temperature, pores and inclusions can be reduced, grains can be refined, a uniform organizational structure can be formed, and good formability can be achieved. As an example, the refining temperature is 450°C, 455°C, 460°C, 465°C, 470°C, 475°C, 480°C, 485°C or 490°C, but is not limited thereto. On the other hand, the above refining time helps to improve the crystal structure of the zinc alloy and improve its mechanical properties and corrosion resistance. If the refining time is too long, it may cause the metal grains to grow too large, thereby reducing the performance of the alloy. As an example, the refining time is 15min, 18min, 20min, 22min, 25min, 28min or 30min.

[0045] In some preferred embodiments of the present application, the furnace treatment further includes: standing for 15 to 25 minutes after refining. Standing can make the residual gas in the melt float and overflow, thereby achieving the purpose of eliminating bubbles; it can also make the zinc alloy grains gradually grow until they are uniform and stable; in addition, the above-mentioned standing process can also release the stress in the zinc alloy, further improving its processing performance.

[0046] In some embodiments of the present application, the zinc alloy melt after the in-furnace treatment begins to flow at 430-460°C and performs online treatment, wherein the online treatment includes: passing the melt through an online filter box and a front box in sequence. That is, the zinc alloy melt after the in-furnace treatment is discharged from the in-furnace treatment equipment within the above temperature range, and performs subsequent purification treatments such as filtration. The melt after purification enters the front box, which can store the melt and adjust the flow state of the melt to make it stable and uniform, so as to facilitate its subsequent uniform introduction into the continuous casting device, thereby improving the efficiency of continuous casting and product quality.

[0047] In some embodiments of the present application, the online filter box uses plate filtration, and the filter plate of the plate filtration is 40 to 60 meshes, which can effectively remove oxides, sulfides, gases and other impurities in the metal melt and improve the purity of the melt. Preferably, the online filter box is a double-plate filter, which has a particularly significant effect on improving the purity of the melt.

[0048] In the above step S2, the purified zinc alloy melt is cast by a continuous casting method at a casting speed of 0.5 to 2 m / min at a casting temperature of 400 to 440° C. Casting at this speed is beneficial to improving the surface quality of the casting and will not cause defects such as pores and shrinkage cavities inside the casting, which will affect the quality of the casting.

[0049] In some embodiments of the present application, the thickness of the zinc alloy ingot is 6 to 10 mm. Preferably, the manufacturing efficiency of the zinc alloy ingot is ≥ 8 t / h, which can achieve both high zinc alloy quality and casting effect.

[0050] In order to further improve the grain fineness and surface quality of the zinc alloy, in some embodiments of the present application, the cooling rate of the casting is ≥80°C / s, preferably, the cooling rate is ≥100°C / s, which is not only conducive to ensuring that the finished plate structure is uniform and fine, but also conducive to improving the strength of the zinc alloy plate and strip. In some preferred embodiments of the present application, the cooling rate of the casting is 100°C / s-120°C / s, which has a significant effect on refining the plate structure and improving the strength, and is easy to achieve. Exemplarily, the cooling rate of the casting is 100°C / s, 105°C / s, 110°C / s, 115°C / s or 120°C / s.

[0051] In the above step S3, the ingot is cold rolled to obtain a zinc alloy sheet and strip. In some embodiments of the present application, in order to further improve the surface quality and formability of the zinc alloy finished product, the pass deformation of the cold rolling is ≥40%. As an example, the pass deformation can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90% or more, but is not limited thereto. In order to achieve a predetermined thickness, multiple passes of rolling can be performed.

[0052] In some embodiments of the present application, the zinc alloy sheet strip has a thickness of 0.5 to 1.5 mm, has stable surface quality, good formability, and is easy to use.

[0053] According to some typical embodiments of the present application, a zinc alloy sheet strip is provided, and the zinc alloy sheet strip is prepared by any one of the above-mentioned preparation methods.

[0054] The present application optimizes the composition of zinc alloy sheets and strips and combines them with appropriate preparation processes to make the prepared zinc alloy sheets and strips have uniform and fine structures, greatly improve the forming performance of the sheets and strips, and solve the problems of unstable surface quality and forming performance of current aluminum alloy sheets or strips.

[0055] In some embodiments of the present application, the average grain size of each region of the zinc alloy sheet and strip is ≤15um, the sheet has a high density, and is free of defects such as pores and looseness.

[0056] In some embodiments of the present application, the tensile strength of the zinc alloy sheet and strip is ≥160MPa, the yield strength is ≥100MPa, the elongation is ≥85%, and the cupping value is ≥10mm, which meets the technical requirements for zinc alloy sheet and strip with high formability.

[0057] According to another typical embodiment of the present application, there is provided an application of any of the above-mentioned zinc alloy sheet and strip materials as a building facade. The present application optimizes the composition of the zinc alloy sheet and strip materials and combines a suitable preparation process to make the prepared zinc alloy sheet and strip materials uniform and fine in structure, greatly improving the forming performance of the sheet and strip materials, and making them particularly suitable for building facades, such as curtain walls.

[0058] The following will further illustrate the technical effects that can be achieved by the present application in combination with embodiments and comparative examples.

[0059] Example 1

[0060] Provided are a high-formability zinc alloy sheet and strip and a preparation method thereof, wherein the alloy composition is as follows: Cu=0.19%; Mn=0.007%; Al=2.53%; Ti=0.12%; La=0.08%; Ce=0.19%, Er=0.12%, Sc=0.08%, and the balance of Zn and unavoidable impurities. The preparation method comprises the following steps:

[0061] S1. Alloy smelting and melt treatment in the furnace: add the pure zinc ingot and other master alloys or additives prepared in proportion into the smelting furnace, mix them evenly, and heat them to melt into liquid zinc melt. The smelting temperature is 505°C. The refining adopts the powder spraying refining method to blow high-purity inert gas into the melt. The refining temperature is 485°C, the time is 25 minutes, and then it is left to stand for 20 minutes.

[0062] S2. Online melt treatment: When the zinc melt temperature reaches 450°C, it starts to discharge. The melt passes through the online filter box and the front box in sequence. The online filter box uses double-plate filtration, and the filter plates are 40 mesh and 60 mesh respectively.

[0063] S3. Casting: The continuous casting method is used to prepare the casting billet, the casting temperature is 420°C, the production speed is 1.2m / min, the thickness of the zinc alloy casting billet is 8mm, the production efficiency is 10t / h, and the casting cooling rate is 105°C / s;

[0064] S4. Rolling: The zinc alloy cast billet is subjected to multiple cold rolling passes to obtain a finished zinc alloy sheet with a thickness of 0.8 mm, wherein the deformation amount of the cold rolling pass is 50%.

[0065] The metallographic photograph (50X) of the finished zinc alloy sheet is as follows Figure 1 As shown, the film photo (200X) is as follows Figure 2 As shown in the figure, it can be seen that the grains are uniform, there are no obvious defects, and the surface quality is excellent.

[0066] The zinc alloy sheet produced by this composition and process has an average grain size of 8.7um in each area, a high density, and no defects such as pores and looseness. The sheet has a tensile strength of 185MPa, a yield strength of 113MPa, an elongation of 92%, and a cupping value of 15mm, meeting the technical requirements for zinc alloy sheets and strips with high formability.

[0067] Example 2

[0068] Provided are a high-formability zinc alloy sheet and strip and a preparation method thereof, wherein the alloy composition is as follows: Cu = 0.1%; Mg = 0.002%; Al = 4.63%; Ti = 0.06%; La = 0.024%; Ce = 0.035%, and the balance is Zn and unavoidable impurities. The preparation method comprises the following steps:

[0069] S1. Alloy smelting and melt treatment in the furnace: add the pure zinc ingot and other master alloys or additives prepared in proportion into the smelting furnace, mix them evenly, and heat them to melt into liquid zinc melt, wherein the smelting temperature is 485°C, and the refining adopts the powder spraying refining method by blowing high-purity inert gas into the melt, the refining temperature is 470°C, the time is 20 minutes, and then it is left to stand for 20 minutes;

[0070] S2. Online melt treatment: When the zinc melt temperature reaches 435°C, it starts to discharge. The melt passes through the online filter box and the front box in sequence. The online filter box uses double-plate filtration, and the filter plates are 40 mesh and 60 mesh respectively.

[0071] S3. Casting: The continuous casting method is used to prepare the casting billet, the casting temperature is 435°C, the production speed is 0.9m / min, the thickness of the zinc alloy casting billet is 8mm, the production efficiency is 8.5t / h, and the casting cooling rate is 102°C / s;

[0072] S4. Rolling: The zinc alloy cast billet is subjected to multiple cold rolling passes to obtain a finished zinc alloy sheet with a thickness of 0.8 mm, wherein the deformation amount of the cold rolling pass is 45%.

[0073] The zinc alloy sheet produced by this composition and process has an average grain size of 10.4um in each area, a high density, and no defects such as pores and looseness. The sheet has a tensile strength of 179MPa, a yield strength of 110MPa, an elongation of 87%, and a cupping value of 14mm, meeting the technical requirements for zinc alloy sheets and strips with high formability.

[0074] Example 3

[0075] Provided are a high-formability zinc alloy sheet and strip and a preparation method thereof, wherein the alloy composition is as follows: Cu = 0.27%; Mn = 0.001%; ​​Al = 0.76%; Ti = 0.18%; Er = 0.25%, and the balance of Zn and unavoidable impurities. The preparation method comprises the following steps:

[0076] S1. Alloy smelting and melt treatment in the furnace: add the pure zinc ingot and other master alloys or additives prepared in proportion into the smelting furnace, mix them evenly, and heat them to melt into liquid zinc melt. The smelting temperature is 465°C. The refining adopts the powder spraying refining method to blow high-purity inert gas into the melt. The refining temperature is 455°C, the time is 30 minutes, and then it is left to stand for 25 minutes.

[0077] S2. Online melt treatment: When the zinc melt temperature reaches 440℃, it starts to discharge. The melt passes through the online filter box and the front box in sequence. The online filter box uses double-plate filtration, and the filter plates are 40 mesh and 60 mesh respectively.

[0078] S3. Casting: The continuous casting method is used to prepare the ingot, the casting temperature is 405°C, the production speed is 1.6m / min, the thickness of the zinc alloy ingot is 8mm, the production efficiency is 10.5t / h, and the casting cooling rate is 105°C / s;

[0079] S4. Rolling: The zinc alloy cast billet is subjected to multiple cold rolling passes to obtain a finished zinc alloy sheet with a thickness of 0.8 mm, wherein the deformation amount of the cold rolling pass is 47%.

[0080] The zinc alloy sheet produced by this composition and process has an average grain size of 12.7um in each area, a high density, and no defects such as pores and looseness. The sheet has a tensile strength of 167MPa, a yield strength of 103MPa, an elongation of 86.8%, and a cupping value of 12mm, meeting the technical requirements for zinc alloy sheets and strips with high formability.

[0081] Example 4

[0082] The difference from Example 1 is that in step S1, the refining temperature is 450°C.

[0083] Example 5

[0084] The difference from Example 1 is that in step S1, the refining temperature is 500°C.

[0085] Example 6

[0086] The difference from Example 1 is that in step S3, the casting temperature is 440°C.

[0087] Example 7

[0088] The difference from Example 1 is that in step S3, the casting temperature is 400°C.

[0089] Example 8

[0090] The difference from Example 1 is that in step S3, the casting speed is 0.5 m / min.

[0091] Example 9

[0092] The difference from Example 1 is that in step S3, the casting speed is 2 m / min.

[0093] Example 10

[0094] The difference from Example 1 is that in step S3, the casting cooling rate is 80°C / s.

[0095] Embodiment 11

[0096] The difference from Example 1 is that in step S3, the casting cooling rate is 70°C / s.

[0097] Example 12

[0098] The difference from Example 1 is that in step S3, the casting cooling rate is 115°C / s.

[0099] Example 13

[0100] The difference from Example 1 is that in step S4, the reduction ratio of the cold rolling pass is 35%.

[0101] Comparative Example 1

[0102] The difference from Example 1 is that the composition of the alloy is different, and the specific composition is as follows: Cu=0.19%; Mn=0.007%; Al=2.53%; Ti=0.12%, and the balance is Al and inevitable impurities.

[0103] The comparative example does not add rare earth elements based on the alloy composition of Example 1, and other preparation processes remain unchanged. The average grain size of each region of the prepared zinc alloy sheet is 19.4um, the tensile strength is 147MPa, the yield strength is 93MPa, the elongation is 75.9%, and the cupping value is 7.9mm.

[0104] It can be seen from the above performance test data that the alloy plates without rare earth elements have larger grains, which directly affects their mechanical properties and cannot meet the technical requirements of zinc alloy plates and strips with high formability.

[0105] Comparative Example 2

[0106] The difference from Example 1 is that after alloy smelting and melt treatment in the furnace in step S1, S2 is skipped and step S3 is performed directly. The casting process of step S3 is as follows: the alloy melt is directly poured into a preheated iron mold, and cooled by circulating water cooling the outer wall of the mold. The cooling rate is only about 150°C / h, the production efficiency is 2.5t / h, and the size of the prepared zinc alloy ingot is 1m(L)*0.5m(W)*0.3m(H); the rolling process of step S4 is as follows: the prepared ingot is subjected to multiple passes of cold rolling, the deformation of the plate in each cold rolling pass is 5%, and the thickness of the prepared plate is 0.8mm.

[0107] The zinc alloy sheet prepared by this method has a tensile strength of 124 MPa, a yield strength of 79 MPa, an elongation of 60.2%, and a cupping value of 5.6 mm, which cannot meet the technical requirements for zinc alloy sheet and strip materials with high formability.

[0108] This comparative example is based on the alloy composition prepared in Example 1, and is cast by a traditional metal mold gravity casting method. It is not filtered online before casting. The cast blank is processed by milling and other machining methods to prepare a zinc alloy cast blank of a certain specification, and then rolled into a zinc alloy plate. The cold rolling pass deformation of the plate is about 5%. The zinc alloy plate prepared by this process has many randomly distributed pores, looseness, slag inclusions and other defects inside, and the plate has low density; because the cooling rate is much lower than the cooling rate of 100℃ / s, the grains and compounds grow significantly during the solidification process, and even after rolling and crushing, they are still relatively coarse, and the average grain size of the plate is 29.7um; the production efficiency is also low due to the influence of cooling intensity, which increases the production cost; due to the poor quality of the cast blank, the plate cannot use a large pass deformation during the rolling process. If the deformation increases, obvious cracks, surface scratches and even broken belts will appear, which greatly reduces the production efficiency and yield rate.

[0109] Comparative Example 3

[0110] The difference from Example 1 is that the content of Al in the prepared alloy composition is 0.3%.

[0111] Comparative Example 4

[0112] The difference from Example 1 is that the prepared alloy composition does not contain titanium.

[0113] Comparative Example 5

[0114] The difference from Example 1 is that the content of Ti in the prepared alloy composition is 0.3%.

[0115] Comparative Example 6

[0116] The difference from Example 1 is that in step S3, the casting temperature is 380°C.

[0117] Comparative Example 7

[0118] The difference from Example 1 is that the casting temperature in step S3 is 450°C.

[0119] The zinc alloy sheets and strips prepared in the above examples and comparative examples were tested, and the test results are listed in Table 1 below.

[0120] Among them, average grain size: refer to the standard "GB / T 6394-2017 Metal Average Grain Size Test Method" to conduct grain size analysis;

[0121] Tensile strength, yield strength and elongation: refer to standard GB / T 228.1-2021 for mechanical properties test and analysis.

[0122] Cupping value: refer to standard GB / T 4156 to test and analyze the cupping value of the plate.

[0123] Table 1

[0124]

[0125]

[0126] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: by optimizing the composition of zinc alloy sheet and strip, combined with a suitable preparation process, the prepared zinc alloy sheet and strip has a uniform and fine structure, greatly improving the forming performance of the sheet and strip, and solving the problem of unstable surface quality and forming performance of the current aluminum alloy sheet or strip. Among them, by regulating the smelting and melt treatment process, the purity of the melt is improved, the looseness, pores and other defects inside the ingot are eliminated, and the metallurgical quality of the ingot is guaranteed; further, in view of the outstanding problem of low production efficiency caused by insufficient cooling intensity in the current preparation of zinc alloy ingots by metal mold gravity casting, the present invention adopts a continuous casting method to prepare zinc alloy ingots, and the cooling intensity of the casting process is high, which improves the production efficiency of the ingot.

[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a zinc alloy sheet strip, characterized in that: The zinc alloy sheet and strip is composed of the following components by mass percentage: Al is 0.5% to 5%, Cu is 0.05% to 0.3%, Ti is 0.05% to 0.2%, Mn is ≤ 0.01%, one or more of the rare earth elements La, Ce, Sc and Er, the content of each rare earth element is 0.01% to 0.3%, and the balance is Zn and unavoidable impurities. The preparation method comprises: Step S1, mixing and smelting raw materials according to the composition of the zinc alloy sheet and strip to obtain a liquid zinc alloy melt, and subjecting the liquid zinc alloy melt to in-furnace treatment and online treatment to obtain a purified zinc alloy melt; Step S2, casting the purified zinc alloy melt by a continuous casting method at a casting temperature of 400-440° C. to prepare a zinc alloy casting billet; Step S3, cold rolling the ingot to obtain the zinc alloy sheet strip.

2. The preparation method according to claim 1, characterized in that: The zinc alloy sheet and strip is composed of the following components by mass percentage: Al is 0.75% to 4.65%, Cu is 0.1% to 0.27%, Ti is 0.06% to 0.18%, Mn≤0.01%, one or more of the rare earth elements La, Ce, Sc and Er, the content of each rare earth element is 0.01% to 0.25%, and the balance is Zn and unavoidable impurities.

3. The preparation method according to claim 1 or 2, characterized in that: In the step S1, the smelting temperature is 460-520°C.

4. The preparation method according to claim 1 or 2, characterized in that: The in-furnace treatment includes using a powder spray refining method to blow a refining agent into the melt through a high-purity inert gas for refining; The refining temperature is 450-490°C and the refining time is 15-30 minutes; Preferably, the in-furnace treatment further comprises: standing still for 15 to 25 minutes after the refining is completed.

5. The preparation method according to claim 1 or 2, characterized in that: The zinc alloy melt after the treatment in the furnace begins to discharge at 430-460° C. to perform the online treatment; The online processing comprises: passing the melt through an online filter box and a front box in sequence; Preferably, the online filter box uses plate filtration, and the filter plate of the plate filtration is 40 to 60 meshes; Preferably, the online filter box is a double-plate filter.

6. The preparation method according to claim 1 or 2, characterized in that: In step S2, the casting speed is 0.5-2 m / min; The thickness of the zinc alloy casting billet is 6 to 10 mm. Preferably, the manufacturing efficiency of the zinc alloy casting billet is ≥ 8 t / h; The cooling rate of the casting is ≥80°C / s, preferably, the cooling rate is ≥100°C / s.

7. The preparation method according to claim 1 or 2, characterized in that: In step S3, the cold rolling pass deformation is ≥40%; Preferably, the zinc alloy sheet strip has a thickness of 0.5 to 1.5 mm.

8. A zinc alloy sheet strip, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 7.

9. The zinc alloy sheet strip according to claim 8, characterized in that: The zinc alloy sheet and strip has an average grain size of ≤15 μm, a tensile strength of ≥160 MPa, a yield strength of ≥100 MPa, an elongation of ≥85%, and a cupping value of ≥10 mm.

10. Use of the zinc alloy sheet strip according to claim 8 or 9 as a building facade.