Scandium-containing spray-formed low-density high-strength aluminum-lithium alloy and preparation method thereof
By using scandium-containing jet forming process in aluminum-lithium alloy, combining high-content Li and Mg elements, adding Cu, Zn, Mn and Sc elements, and using nano-scale Al3 (Sc, Zr) particles, aluminium lithium in traditional casting was solved. It is difficult for alloys to take into account both the problems of low density and high strength, and achieve efficient aluminum-lithium alloy preparation, with excellent mechanical properties and density.
Patent Information
- Application Number
- CN202410911459.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional casting processes are difficult to take into account both low density and high strength in aluminum-lithium alloys. When the lithium addition amount exceeds 4.2%, it will lead to segregation and brittle fracture, affecting the weight loss effect.
Using scandium-containing jet forming process, the density is reduced by high content of Li and Mg elements, and the δ'(Al3Li) precipitated phase is precipitated in the crystal to improve the intensity, and the addition of Cu, Zn, Mn and Sc elements is improved to improve the opposite sex and grain refinement. , nanoscale Al3 (Sc, Zr) particles are used to inhibit recrystallization and slippage, and the rapid solidification technology is combined to avoid element segregation.
The combination of low density and high strength is achieved, the density of aluminum-lithium alloy is reduced, and the tensile strength and yield strength are significantly improved, the elongation is increased, the grains are small, and the density is high, which solves the problem of solid solubility limit and segregation in traditional casting.
Smart Images

Figure FDA0004933728400000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy formulation and preparation process, and in particular relates to a low-density, high-strength aluminum-lithium alloy and a preparation method thereof. Background Art
[0002] The density of lithium (Li) is only 0.534g / cm 3 , is the lightest metal in nature. When 1wt.% of lithium is added to aluminum alloy, the density can be reduced by 3% and the elastic modulus can be increased by about 6%. At the same time, the addition of lithium can also improve the strength and damage tolerance of aluminum alloys. Aluminum-lithium alloys can achieve all-round weight reduction. Therefore, aluminum-lithium alloys are considered to be one of the most competitive lightweight and high-strength structural materials in the 21st century. Structures made of aluminum-lithium alloys can achieve a weight reduction of more than 10% and a stiffness increase of more than 15% compared to traditional aluminum alloys.
[0003] However, it is difficult to further achieve a good match between low density and high strength of aluminum-lithium alloys under traditional casting process conditions. To further improve the weight reduction effect of aluminum-lithium alloys, it is usually at the expense of their strength. The main reason is that when the lithium addition exceeds the solid solubility of 4.2% during the casting process, severe segregation will occur at the grain boundaries. In addition, reducing the density by increasing the lithium content will cause more coherent δ'(Al3Li) metastable phases with a small mismatch with the matrix to precipitate in the alloy. The coplanar slip characteristics of the δ'(Al3Li) phase will cause stress concentration at the grain boundaries, thereby causing brittle fracture.
[0004] Therefore, in order to further reduce the density of aluminum-lithium alloys while ensuring that the alloy has good strength, it is necessary to specially develop a low-density and high-strength aluminum-lithium alloy composition formula and solve the segregation problem existing in the alloy. Summary of the invention
[0005] In view of the problem that low density and high strength of aluminum-lithium alloys cannot be achieved in the prior art, the present invention provides a low-density and high-strength aluminum-lithium alloy component formula, which achieves high strength while further reducing the density of the aluminum-lithium alloy. The present invention also provides a preparation method of the low-density and high-strength aluminum-lithium alloy.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] In the first aspect, the present invention provides a scandium-containing injection-formed low-density high-strength aluminum-lithium alloy, which is composed of, by mass percentage: Li 3.0-8.5%, Mg 1.0-6.5%, Cu 0.1-1.0%, Mn 0.05-0.50%, Zn 0.1-0.50%, Zr 0.05-0.30%, Sc 0.1-0.60%, the total amount of impurity elements Fe, Si, Na, and K is less than 0.25%, of which Fe is less than 0.15%, Si is less than 0.10%, and the balance is Al, and the total mass percentage is 100%.
[0008] The invention provides a spray-formed low-density high-strength aluminum-lithium alloy containing scandium, wherein the high content of Li and Mg elements can reduce the density of the aluminum alloy, and at the same time, a large number of δ' (Al3Li) precipitation phases are precipitated in the crystal to improve the strength of the aluminum-lithium alloy. Cu and Zn elements are added to further improve the strength of the aluminum-lithium alloy. Mn elements are added to improve the anisotropy of the aluminum-lithium alloy.
[0009] The present invention provides a spray-formed low-density and high-strength aluminum-lithium alloy containing scandium. The rare earth element Sc is added to the alloy to play four roles: first, it can significantly refine the grains, and simultaneously improve the strength and plasticity of the alloy under the action of the fine grain strengthening mechanism; second, the nanometer-scale Al3 (Sc, Zr) particles precipitated by the combined addition of Sc and Zr can inhibit the recrystallization of the material during thermal deformation and heat treatment; third, the nanometer-scale Al3 (Sc, Zr) particles precipitated by the combined addition of Sc and Zr have a good strengthening effect; fourth, the formed composite strengthening particles Al3 (Sc, Zr, Li) with Al3 (Sc, Zr) as the core can stimulate multi-system slip, making up for the deficiency of metastable δ' (Al3Li) coplanar slip.
[0010] The spray forming preparation method adopted by the present invention belongs to the rapid solidification technology, which can break through the solid solubility of alloy elements in the solid solution under equilibrium conditions and will not cause element segregation.
[0011] More preferably, the Li is 99.9% pure lithium, the Cu is 99.9% pure copper, the Zn is 99.9% pure zinc, the Mn is an Al-Mn master alloy, the Zr is an Al-Zr master alloy, and the Sc is an Al-Sc master alloy.
[0012] More preferably, the Al-Mn master alloy is an Al-10Mn master alloy, the Al-Zr master alloy is an Al-5Zr master alloy, and the Al-Sc master alloy is an Al-5Sc master alloy.
[0013] In a second aspect, in order to achieve the above object, the present invention also provides a method for preparing the above low-density and high-strength aluminum-lithium alloy, which comprises the following steps:
[0014] (1) Alloy configuration: raw materials are configured according to mass percentages of 3.0-8.5% Li, 1.0-6.5% Mg, 0.1-1.0% Cu, 0.1-0.50% Zn, 0.05-0.50% Mn, 0.05-0.30% Zr, 0.1-0.6% Sc, and the balance is Al; wherein Al is 99.90% pure aluminum, Mg is 99.9% pure magnesium, Li is 99.9% pure lithium, Cu is 99.9% pure copper, Zn is 99.9% pure zinc, Mn is Al-10Mn master alloy, Zr is Al-5Zr master alloy, and Sc is Al-5Sc master alloy;
[0015] (2) Alloy smelting: Put the prepared pure Al, pure Cu and pure Zn into a medium frequency induction melting furnace, turn on the argon protection, and heat until the pure Al, pure Cu and pure Zn are melted. When the melt temperature rises to 750-770°C, add Al-10Mn, Al-5Zr and Al-5Sc intermediate alloys. Use electromagnetic stirring, and heat the melt to 810-830°C, keep it warm for 2-3 hours and then cool it down. When the melt temperature drops to 720-740°C, add pure magnesium, use electromagnetic stirring and keep it warm for 1-2 hours. After keeping warm, maintain 720-740°C and add pure Li, use electromagnetic stirring and keep it warm for 1-2 hours. After keeping warm, the completely molten aluminum alloy melt is refined in the temperature range of 690-740°C;
[0016] (3) Spray forming ingot making: The smelted aluminum alloy melt is filtered with an aluminum plate and then transferred to a ladle; the liquid metal in the ladle is atomized into liquid particles with nitrogen, wherein the atomization pressure is 0.4-1.2 MPa and the atomization gas flow rate is 0.4-0.8 m 3 / min; atomized melt particles are deposited on a deposition disk with a diameter of 300-800 mm by scanning spray deposition with double nozzles, wherein the nozzle scanning frequency is 7-15 Hz, the rotation speed of the deposition disk is 55-100 rpm, and the deposition height is 500-1000 mm; the solid H content in the obtained ingot is less than 0.5 cm 3 / 100g, density is greater than 97%, and average grain size is less than 70μm.
[0017] (4) Extrusion and blanking: The spray-formed aluminum-lithium alloy ingot obtained above is machined, the head and tail are cut, and the surface oxide layer is removed by peeling. The machined ingot is preheated, and the preheated ingot is put into an extruder for extrusion and blanking, and extruded into a slab with a thickness of 150 mm.
[0018] (5) Rolling: The extruded slab is subjected to multiple hot rolling steps to be rolled into a finished plate.
[0019] (6) Heat treatment: The rolled plate is kept at 460°C for 1 hour and then immediately quenched in water at room temperature; aged at 120°C for 12 hours within 4 hours after quenching, and naturally cooled to room temperature after aging to obtain a low-density and high-strength aluminum-lithium alloy product.
[0020] Further preferably, the smelting furnace in step (2) is a medium frequency induction furnace.
[0021] More preferably, the preheating temperature of the ingot after machining in step (4) is 420-460°C.
[0022] More preferably, the extrusion temperature in step (4) is 420-460°C.
[0023] More preferably, the hot rolling temperature in step (5) is 420-460°C.
[0024] More preferably, the deformation amount of each hot rolling in step (5) is 5% to 10%.
[0025] The scandium-containing spray-formed low-density high-strength aluminum-lithium alloy of the present invention has both low density and high strength.
[0026] The advantages and beneficial effects of the present invention are:
[0027] (1) Compared with the existing mature aluminum-lithium alloys, the low-density and high-strength aluminum-lithium alloy of the present invention has higher lithium and magnesium contents, which can significantly reduce the density of the aluminum alloy. At the same time, the higher lithium content can cause more δ' (Al3Li) strengthening phases to precipitate during the subsequent aging process. At the same time, the combined addition of Cu and Zn further improves the strength of the aluminum-lithium alloy, and the addition of Mn reduces the anisotropy. At the same time, the microalloying elements scandium and zirconium added to the aluminum-lithium alloy of the present invention have higher contents, which can further refine the grains. At the same time, the nanoscale Al3 (Sc, Zr) phase precipitated by the combined addition of Sc and Zr can further improve the strength of the invented aluminum-lithium alloy and improve the coplanar slip problem of the δ' phase.
[0028] (2) The rapid solidification spray forming process breaks through the limit of the solid solution content of the traditional cast aluminum alloy. The composition is uniform, there is no obvious macro-segregation, the grains are fine, and the H content is low, which is conducive to the preparation of high-quality aluminum-lithium alloy ingots.
[0029] (3) The aluminum-lithium alloy prepared by the spray forming method of the present invention has an average grain size of less than 70 μm and a density of less than 2.4 g / cm 3 , tensile strength greater than 550MPa, yield strength greater than 450MPa, and elongation greater than 7%. The alloy reduces the density of the alloy while increasing its strength. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] A scandium-containing spray-formed low-density high-strength aluminum-lithium alloy, the components and mass percentages of which are: Li content 3.6%, Mg content 2.0%, Cu content 0.3%, Mn content 0.25%, Zn content 0.25%, Zr content 0.25%, Sc content 0.5%, and the balance Al.
[0033] A method for preparing a spray-formed low-density and high-strength aluminum-lithium alloy containing scandium, the specific steps are as follows:
[0034] (1) Alloy configuration: The alloy is weighed according to the above-mentioned alloy chemical composition and weight percentage, wherein Al is 99.90% high-purity aluminum, Mg is 99.9% pure magnesium, Cu is 99.9% pure copper, Zn is 99.9% pure zinc, Mn is Al-10Mn master alloy, Zr is Al-5Zr master alloy, and Sc is Al-5Sc master alloy.
[0035] (2) Alloy smelting: Put the weighed pure Al, pure Cu and pure Zn raw materials into a medium-frequency induction furnace protected by argon, and heat them until the metal is melted. When the melt temperature rises to 755°C, add Al-10Mn, Al-5Zr and Al-5Sc intermediate alloys. After electromagnetic stirring, raise the melt temperature to 818°C, keep it warm for 3 hours and then cool it down. When the melt temperature drops to 726°C, add pure magnesium raw materials, stir it electromagnetically and keep it warm for 1.5 hours. After keeping it warm, add pure Li at 725-730°C, stir it electromagnetically and keep it warm for 1.5 hours. After keeping it warm, refine the completely molten aluminum alloy melt in the range of 700-710°C.
[0036] (3) Spray forming ingot making: The smelted aluminum alloy melt is filtered with an aluminum plate and then transferred to a ladle; the liquid metal in the ladle is atomized into liquid particles with nitrogen, wherein the atomization pressure is 0.5 MPa and the atomization gas flow rate is 0.6 m 3 / min; the atomized melt particles were deposited on a deposition disk with a diameter of 500 mm by scanning spray deposition with a double nozzle, wherein the nozzle scanning frequency was 8.5 Hz, the rotation speed of the deposition disk was 60 rpm, and the deposition height was 750 mm; the solid H content in the obtained ingot was 0.3 cm 3 / 100g, density is 98.0%, and average grain size is 60μm.
[0037] (4) Extrusion and blanking: The spray-formed aluminum-lithium alloy ingot obtained above is machined, the head and tail are cut, and the surface oxide layer is removed by peeling. The machined ingot is preheated at a temperature of 430°C, and the preheated ingot is put into an extruder for extrusion and blanking at a temperature of 440°C, and extruded into a slab with a thickness of 150 mm.
[0038] (5) Extrusion billet: The extruded slab is rolled three times at a rolling temperature of 447°C and a deformation of 8% in each pass to form a slab of 116.8 mm.
[0039] (6) The rolled plate is kept at 460°C for 1 hour, and then immediately quenched in water at room temperature; aged at 120°C for 12 hours within 4 hours after quenching, and naturally cooled to room temperature after aging. The density of the heat-treated plate is tested and a room temperature tensile test is performed. The results show that the density of the aluminum-lithium alloy obtained according to the above formula and preparation method is 2.36 g / cm 3 , the tensile strength is 563.5MPa, the yield strength is 472.5MPa, and the elongation is 8.5%.
[0040] Example 2
[0041] A spray-formed low-density high-strength aluminum-lithium alloy containing scandium has the following components and mass percentages: Li content 4.0%, Mg content 1.0%, Cu content 0.1%, Zn content 0.20%, Mn content 0.1%, Zr content 0.15%, Sc content 0.3%, and the balance Al.
[0042] A method for preparing a spray-formed low-density and high-strength aluminum-lithium alloy containing scandium, the specific steps are as follows:
[0043] (1) Alloy configuration: The alloy is weighed according to the above-mentioned alloy chemical composition and weight percentage, wherein Al is 99.90% high-purity aluminum, Mg is 99.9% pure magnesium, Cu is 99.9% pure copper, Zn is 99.9% pure zinc, Mn is Al-10Mn master alloy, Zr is Al-5Zr master alloy, and Sc is Al-5Sc master alloy.
[0044] (2) Alloy smelting: Put the weighed pure Al, pure Cu and pure Zn raw materials into a medium-frequency induction furnace protected by argon, and heat them until the metal is melted. When the melt temperature rises to 760°C, add Al-10Mn, Al-5Zr and Al-5Sc intermediate alloys. After electromagnetic stirring, raise the melt temperature to 820°C, keep it warm for 2.5 hours and then cool it down. When the melt temperature drops to 730°C, add pure magnesium raw materials, stir it electromagnetically and keep it warm for 1 hour. After keeping it warm, add pure Li at 720-725°C, stir it electromagnetically and keep it warm for 1 hour. After keeping it warm, refine the completely molten aluminum alloy melt in the range of 690-695°C.
[0045] (3) Spray forming ingot making: The smelted aluminum alloy melt is filtered with an aluminum plate and then transferred to a ladle; the liquid metal in the ladle is atomized into liquid particles with nitrogen, wherein the atomization pressure is 1.0 MPa and the atomization gas flow rate is 0.7 m 3 / min; the atomized melt particles were deposited on a deposition disk with a diameter of 600 mm by scanning spray deposition with a double nozzle, wherein the nozzle scanning frequency was 9.0 Hz, the rotation speed of the deposition disk was 85 rpm, and the deposition height was 550 mm; the solid H content in the obtained ingot was 0.35 cm 3 / 100g, density is 98.70%, and average grain size is 55μm.
[0046] (4) Extrusion and blanking: The spray-formed aluminum-lithium alloy ingot obtained above is machined, the head and tail are cut, and the surface oxide layer is removed by peeling. The machined ingot is preheated at a temperature of 435°C, and the preheated ingot is put into an extruder for extrusion and blanking at a temperature of 445°C, and extruded into a slab with a thickness of 150 mm.
[0047] (5) Extrusion billet: The extruded slab is rolled three times at a rolling temperature of 455°C and a deformation of 8% in each pass to form a slab of 116.8 mm.
[0048] (6) The rolled plate is kept at 460°C for 1 hour, and then immediately quenched in water at room temperature; aged at 120°C for 12 hours within 4 hours after quenching, and naturally cooled to room temperature after aging. The density of the heat-treated plate is tested and a room temperature tensile test is performed. The results show that the density of the aluminum-lithium alloy obtained according to the above formula and preparation method is 2.31 g / cm 3 , the tensile strength is 575.6MPa, the yield strength is 462.8MPa, and the elongation is 7.8%.
[0049] Example 3
[0050] A spray-formed low-density high-strength aluminum-lithium alloy containing scandium has the following components and mass percentages: Li content 5.1%, Mg content 3.0%, Cu content 0.15%, Zn content 0.43%, Mn content 0.3%, Zr content 0.2%, Sc content 0.4%, and the balance Al.
[0051] A method for preparing a spray-formed low-density and high-strength aluminum-lithium alloy containing scandium, the specific steps are as follows:
[0052] (1) Alloy configuration: The alloy is weighed according to the above-mentioned alloy chemical composition and weight percentage, wherein Al is 99.90% high-purity aluminum, Mg is 99.9% pure magnesium, Cu is 99.9% pure copper, Zn is 99.9% pure zinc, Mn is Al-10Mn master alloy, Zr is Al-5Zr master alloy, and Sc is Al-5Sc master alloy.
[0053] (2) Alloy smelting: Put the weighed pure Al, pure Cu and pure Zn raw materials into a medium frequency induction furnace protected by argon, and heat them until the metal is melted. When the melt temperature rises to 797°C, add Al-10Mn, Al-5Zr and Al-5Sc intermediate alloys. After electromagnetic stirring, raise the melt temperature to 825°C, keep it warm for 2.3 hours and then cool it down. When the melt temperature drops to 736°C, add pure magnesium raw materials, stir it electromagnetically and keep it warm for 1.8 hours. After keeping it warm, add pure Li when maintaining 733-737°C, stir it electromagnetically and keep it warm for 1.8 hours. After keeping it warm, refine the completely molten aluminum alloy melt in the range of 725-727°C.
[0054] (3) Spray forming ingot: The smelted aluminum alloy melt is filtered with an aluminum plate and then transferred to a ladle; the liquid metal in the ladle is atomized into liquid particles with nitrogen, wherein the atomization pressure is 1.1 MPa and the atomization gas flow rate is 0.75 m 3 / min; atomized melt particles were deposited on a deposition disk with a diameter of 700 mm by scanning spray deposition with a double nozzle, wherein the nozzle scanning frequency was 12.0 Hz, the rotation speed of the deposition disk was 93 rpm, and the deposition height was 800 mm; the solid H content in the obtained ingot was 0.27 cm 3 / 100g, density is 97.80%, and average grain size is 64μm.
[0055] (4) Extrusion and blanking: The spray-formed aluminum-lithium alloy ingot obtained above is machined, the head and tail are cut, and the surface oxide layer is removed by peeling. The machined ingot is preheated at a temperature of 450°C, and the preheated ingot is put into an extruder for extrusion and blanking at a temperature of 440°C, and extruded into a slab with a thickness of 150 mm.
[0056] (5) Extrusion billet: The extruded slab is rolled three times at a rolling temperature of 452°C and a deformation of 10% in each pass to form a slab of 109.4 mm.
[0057] (6) The rolled plate is kept at 460°C for 1 hour, and then immediately quenched in water at room temperature; aged at 120°C for 12 hours within 4 hours after quenching, and naturally cooled to room temperature after aging. The density of the heat-treated plate is tested and a room temperature tensile test is performed. The results show that the density of the aluminum-lithium alloy obtained according to the above formula and preparation method is 2.21g / cm 3 , the tensile strength is 592.3MPa, the yield strength is 484.5MPa, and the elongation is 7.4%.
[0058] Example 4
[0059] A scandium-containing spray-formed low-density high-strength aluminum-lithium alloy, the components and mass percentages of which are: Li content 7.9%, Mg content 6.0%, Cu content 0.7%, Zn content 0.5%, Mn content 0.4%, Zr content 0.15%, Sc content 0.1%, and the balance Al.
[0060] A method for preparing a spray-formed low-density and high-strength aluminum-lithium alloy containing scandium, the specific steps are as follows:
[0061] (1) Alloy configuration: The alloy is weighed according to the above-mentioned alloy chemical composition and weight percentage, wherein Al is 99.90% high-purity aluminum, Mg is 99.9% pure magnesium, Cu is 99.9% pure copper, Zn is 99.9% pure zinc, Mn is Al-10Mn master alloy, Zr is Al-5Zr master alloy, and Sc is Al-5Sc master alloy.
[0062] (2) Alloy smelting: Put the weighed pure Al, pure Cu and pure Zn raw materials into a medium-frequency induction furnace protected by argon, and heat them until the metal is melted. When the melt temperature rises to 755°C, add Al-10Mn, Al-5Zr and Al-5Sc master alloys. After electromagnetic stirring, raise the melt temperature to 816°C, keep it warm for 2.2 hours and then cool it down. When the melt temperature drops to 728°C, add pure magnesium raw materials, stir it electromagnetically and keep it warm for 1.2 hours. After keeping it warm, add pure Li when maintaining 723-728°C, stir it electromagnetically and keep it warm for 1.2 hours. After keeping it warm, refine the completely molten aluminum alloy melt in the range of 715-718°C.
[0063] (3) Spray forming ingot making: The smelted aluminum alloy melt is filtered with an aluminum plate and then transferred to a ladle; the liquid metal in the ladle is atomized into liquid particles with nitrogen, wherein the atomization pressure is 0.6 MPa and the atomization gas flow rate is 0.45 m 3 / min; the atomized melt particles were deposited on a deposition disk with a diameter of 350mm by scanning spray deposition with a double nozzle, wherein the nozzle scanning frequency was 7.8Hz, the rotation speed of the deposition disk was 60rpm, and the deposition height was 550mm; the solid H content in the obtained ingot was 0.25cm 3 / 100g, density is 98.20%, and average grain size is 58μm.
[0064] (4) Extrusion and blanking: The spray-formed aluminum-lithium alloy ingot obtained above is machined, the head and tail are cut, and the surface oxide layer is removed by peeling. The machined ingot is preheated at a temperature of 455°C, and the preheated ingot is put into an extruder for extrusion and blanking at a temperature of 458°C, and extruded into a slab with a thickness of 150 mm.
[0065] (5) Extrusion billet: The extruded slab is rolled three times at a rolling temperature of 456°C and a deformation of 5% in each pass to form a slab of 128.6 mm.
[0066] (6) The rolled plate is kept at 460°C for 1 hour, and then immediately quenched in water at room temperature; aged at 120°C for 12 hours within 4 hours after quenching, and naturally cooled to room temperature after aging. The density of the heat-treated plate is tested and a room temperature tensile test is performed. The results show that the density of the aluminum-lithium alloy obtained according to the above formula and preparation method is 1.97g / cm 3 , the tensile strength is 602.4MPa, the yield strength is 510.3MPa, and the elongation is 7.2%.
[0067] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A spray-formed low-density, high-strength aluminum-lithium alloy containing scandium, characterized in that: By mass percentage: The total amount of impurity elements Fe, Si, Na, and K is less than 0.25%; Of which Fe is less than 0.15%; Si is less than 0.10%; The balance is composed of Al.
2. The scandium-containing spray-formed low-density high-strength aluminum-lithium alloy according to claim 1, characterized in that: The Al is 99.90% pure aluminum, the Mg is 99.9% pure magnesium, the Li is 99.9% pure lithium, the Cu is 99.9% pure copper, the Zn is 99.9% pure zinc, the Mn is an Al-Mn master alloy, the Zr is an Al-Zr master alloy, and the Sc is an Al-Sc master alloy.
3. The scandium-containing spray-formed low-density high-strength aluminum-lithium alloy according to claim 2, characterized in that: The Al-Mn master alloy is an Al-10Mn master alloy, the Al-Zr master alloy is an Al-5Zr master alloy, and the Al-Sc master alloy is an Al-5Sc master alloy.
4. A method for preparing a scandium-containing spray-formed low-density high-strength aluminum-lithium alloy as claimed in any one of claims 1 to 3, characterized in that The following steps are involved: (1) Alloy configuration: raw materials are configured according to mass percentages of 3.0-8.5% Li, 1.0-6.5% Mg, 0.1-1.0% Cu, 0.1-0.50% Zn, 0.05-0.50% Mn, 0.05-0.30% Zr, 0.1-0.6% Sc, and the balance is Al; wherein Al is 99.90% pure aluminum, Mg is 99.9% pure magnesium, Li is 99.9% pure lithium, Cu is 99.9% pure copper, Zn is 99.9% pure zinc, Mn is Al-10Mn master alloy, Zr is Al-5Zr master alloy, and Sc is Al-5Sc master alloy; (2) Alloy smelting: put the prepared pure Al, pure Cu and pure Zn into a medium frequency induction melting furnace, turn on the inert gas protection, and heat the pure Al, pure Cu and pure Zn until they are melted; when the melt temperature rises to 750-770°C, add Al-10Mn, Al-5Zr and Al-5Sc master alloys; use electromagnetic stirring, and heat the melt to 810-830°C, keep it warm for 2-3 hours and then cool it down; when the melt temperature drops to 720-740°C, add pure magnesium, use electromagnetic stirring and keep it warm for 1-2 hours; after keeping it warm, add pure Li at 720-740°C, use electromagnetic stirring and keep it warm for 1-2 hours; after keeping it warm, refine the completely molten aluminum alloy melt in the temperature range of 690-740°C; (3) Spray forming ingot making: The smelted aluminum alloy melt is filtered with an aluminum plate and then transferred to a ladle; the liquid metal in the ladle is atomized into liquid particles with nitrogen, wherein the atomization pressure is 0.4-1.2 MPa and the atomization gas flow rate is 0.4-0.8 m 3 / min; atomized melt particles are deposited on a deposition disk with a diameter of 300-800 mm by scanning spray deposition with double nozzles, wherein the nozzle scanning frequency is 7-15 Hz, the rotation speed of the deposition disk is 55-100 rpm, and the deposition height is 500-1000 mm; the solid H content in the obtained ingot is less than 0.5 cm 3 / 100g, density greater than 97%, average grain size less than 70μm; (4) Extrusion and blanking: The spray-formed aluminum-lithium alloy ingot obtained above is machined, the head and tail are cut, and the surface oxide layer is removed by peeling; the machined ingot is preheated, and the preheated ingot is put into an extruder for extrusion and blanking, and extruded into a slab with a thickness of 150 mm; (5) rolling forming: the extruded slab is subjected to multiple hot rolling processes to be rolled into a finished plate; (6) Heat treatment: The rolled plate is kept at 460°C for 1 hour and then immediately quenched in water at room temperature; aged at 120°C for 12 hours within 4 hours after quenching, and naturally cooled to room temperature after aging to obtain a low-density and high-strength aluminum-lithium alloy product.
5. The method for preparing a scandium-containing spray-formed low-density high-strength aluminum-lithium alloy as claimed in claim 4, characterized in that The smelting furnace in step (2) is a medium frequency induction furnace.
6. The method for preparing a scandium-containing spray-formed low-density high-strength aluminum-lithium alloy as claimed in claim 4, characterized in that The preheating temperature of the ingot after machining in step (4) is 420-460°C.
7. The method for preparing a scandium-containing spray-formed low-density high-strength aluminum-lithium alloy as claimed in claim 4, characterized in that The extrusion temperature in step (4) is 420-460°C.
8. The method for preparing a scandium-containing spray-formed low-density high-strength aluminum-lithium alloy as claimed in claim 4, characterized in that The hot rolling temperature in step (5) is 420-460°C.
9. The method for preparing a scandium-containing spray-formed low-density high-strength aluminum-lithium alloy as claimed in claim 4, characterized in that The deformation amount of each hot rolling in step (5) is 5% to 10%.
10. A scandium-containing spray-formed low-density high-strength aluminum-lithium alloy as claimed in claim 1, which has both low density and high strength.
Citation Information
Cited By
High-performance 7075 aluminum alloy plate process and application of high-performance 7075 aluminum alloy plate process in new energy automobile
CN121272273A
A multi-element reinforced high-strength and high-toughness aluminum-lithium alloy with low scandium content
CN122879570A