Preparation method of B4C reinforced aluminum-based composite material

Through the preparation method of B4C reinforced aluminum-based composite material, combined with the mixing of carbon black, tungsten carbide and B4C powder, ball milling and static press forming processes, the problem of insufficient strength and wear resistance of aluminum-based composite material is solved, and high strength, Aluminum-based composite material with high hardness and good wear resistance meets high application needs.

CN118932220APending Publication Date: 2024-11-12NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410968863.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing aluminum-based composite materials have low strength and are difficult to meet the needs of high-load-bearing components. Boron carbide-reinforced aluminum-based composite materials have problems of insufficient brittleness and wear resistance.

Method used

Using the preparation method of B4C reinforced aluminum-based composite material, the mixture and ball mill of atomized Al-Zn-Mg-Cu alloy powder with carbon black, tungsten carbide powder and B4C powder are combined with cold isostatic pressure and hot isostatic pressure forming process , an aluminum-based composite material with high strength, high hardness and good wear resistance was prepared.

Benefits of technology

The high strength, high hardness and good wear resistance of aluminum-based composite materials are achieved, meeting higher comprehensive performance needs, significantly reducing the friction coefficient and wear rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932220A_ABST
    Figure CN118932220A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a B4C reinforced aluminum-based composite material, which is characterized in that carbon black, B4C and tungsten carbide are mixed to reinforce the aluminum-based composite material, amorphous carbon, B4C particles and high-hardness tungsten carbide particles with a self-lubricating effect are introduced into an aluminum alloy, and the aluminum-based composite material with high strength, high hardness and good wear resistance is prepared. Therefore, the composite material has more excellent comprehensive performance and can meet higher application requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention specifically relates to the technical field of composite material preparation, and in particular to a method for preparing a B4C reinforced aluminum-based composite material. Background Art

[0002] Metal matrix composites (MMCs) are made of metal materials as the matrix and continuous fibers, short fibers, whiskers or ceramic particles as the reinforcement phase. According to the type and form of the reinforcement phase, they can be divided into continuous fiber reinforced composites, discontinuous reinforced composites, layered composites, etc. Aluminum and its alloys are one of the most commonly used matrix materials in MMCs, and aluminum alloys or aluminum matrix composites are lightweight composites. Therefore, aluminum matrix composites (AMCs) play an important role in advanced application fields such as automobiles, aerospace and military due to their specific low density, high mechanical properties and low cost. Among them, particle reinforced aluminum matrix composites (Particulate reinforced aluminum matrix composites, PRAMC) are the most mature. PRAMC is favored by more industries, especially in the aerospace field. At present, the more mature aluminum matrix composites are mostly based on Al-Cu-Mg and Al-Mg-Si alloys. The strength of the material is relatively low and it is difficult to meet the requirements of high-load-bearing components. Boron carbide (BC) has high elastic modulus, hardness, excellent chemical stability, good wear resistance and neutron absorption performance, and its density is similar to that of aluminum. Therefore, it has been often used in the preparation of metal-based composites in recent years. However, although it has obvious advantages in reinforcing aluminum-based composites, it is a brittle particle and has defects in reinforcing aluminum-based composites, such as reduced brittleness and insufficient wear resistance, which cannot meet the needs of aluminum-based composites with higher comprehensive performance. Summary of the invention

[0003] Based on the above background, the present invention provides a method for preparing a B4C reinforced aluminum-based composite material.

[0004] The technical solution of the present invention is:

[0005] A method for preparing a B4C reinforced aluminum-based composite material, such as Figure 1 As shown, it includes the following steps:

[0006] S1: Al-Zn-Mg-Cu alloy powder is prepared by atomizing Al powder, Zn powder, Mg powder and Cu powder; the contents of the Al powder, Zn powder, Mg powder and Cu powder are: 85-97wt% of Al powder, 4-5wt% of Zn powder, 1-2wt% of Mg powder and 0.5-1.5wt% of Cu powder respectively;

[0007] S2: taking carbon black and drying it;

[0008] S3: taking tungsten carbide powder and B4C powder, mixing alloy powder, carbon black, tungsten carbide powder and B4C powder, and ball milling under the protection of argon gas;

[0009] S4: The ball-milled powder is subjected to cold isostatic pressing to form an ingot, and the ingot is subjected to vacuum hot isostatic pressing to form an ingot.

[0010] Furthermore, the amount of carbon black in step S2 is 5-15% of the volume of the alloy powder in step S1.

[0011] Furthermore, the amount of tungsten carbide powder in step S3 is 1-5% of the volume of the alloy powder in step S1.

[0012] Furthermore, the amount of B4C powder in step S3 is 10-35% of the volume of the alloy powder in step S1.

[0013] Furthermore, in step S3, zirconium oxide is used as a ball milling medium, the ball-to-material ratio is (2-5):1, and the ball milling speed is lower than 100 r / min.

[0014] Furthermore, the cold isostatic pressing pressure in step S4 is 190-220 MPa, and the holding time is 45-60 min.

[0015] Furthermore, the hot isostatic pressing in step S4 is performed at a temperature of 500-580° C., a pressure of 100-150 MPa, and a holding time of 2-4 hours.

[0016] The effective effects achieved by adopting the present invention are:

[0017] The present invention adopts a carbon black, B4C, tungsten carbide hybrid reinforced aluminum-based composite material, introduces amorphous carbon with self-lubricating effect, B4C particles, and high-hardness tungsten carbide particles into the aluminum alloy, and prepares an aluminum-based composite material with high strength, high hardness and good wear resistance, so that it has more excellent comprehensive performance and can meet higher application requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of the preparation process flow of B4C reinforced aluminum-based composite materials. DETAILED DESCRIPTION

[0019] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0020] Embodiment 1: A method for preparing a B4C reinforced aluminum-based composite material, comprising the following steps:

[0021] S1: Al-Zn-Mg-Cu alloy powder is prepared by atomizing Al powder, Zn powder, Mg powder and Cu powder; the contents of the Al powder, Zn powder, Mg powder and Cu powder are: 92.5wt% of Al powder, 5wt% of Zn powder, 1.5wt% of Mg powder and 1wt% of Cu powder respectively;

[0022] The particle size of Al powder is 10-20μm, the particle size of Cu powder is 5-15μm; the particle size of Mg powder is 15-10μm; the particle size of Zn powder is 5-10μm;

[0023] S2: taking 5% of the volume of the alloy powder in step S1 and drying the carbon black; the particle size of the carbon black is 3-5 μm;

[0024] S3: taking tungsten carbide powder according to 2% of the volume of the alloy powder in step S1, taking B4C powder according to 15% of the volume of the alloy powder in step S1, mixing the alloy powder, carbon black, tungsten carbide powder and B4C powder, and then ball milling under the protection of argon; the particle size of B4C powder is 5-10μm; the particle size of tungsten carbide powder is 0.5-1.5μm;

[0025] During ball milling, zirconium oxide (d = 10 mm) was used as the ball milling medium, the ball-to-material ratio was 5:1, and the ball milling speed was less than 100 r / min;

[0026] S4: The ball-milled powder is subjected to cold isostatic pressing to form an ingot, and the ingot is subjected to vacuum hot isostatic pressing to form an ingot.

[0027] The pressure of cold isostatic pressing in this step is 190-220MPa, and the holding time is 45-60min; the temperature of hot isostatic pressing is 500-580°C, the pressure is 100-150MPa, and the holding time is 2-4h.

[0028] Embodiment 2: A method for preparing a B4C reinforced aluminum-based composite material, comprising the following steps:

[0029] S1: Al-Zn-Mg-Cu alloy powder is prepared by atomizing Al powder, Zn powder, Mg powder and Cu powder; the contents of the Al powder, Zn powder, Mg powder and Cu powder are: 92.5wt% of Al powder, 5wt% of Zn powder, 1.5wt% of Mg powder and 1wt% of Cu powder respectively;

[0030] The particle size of Al powder is 10-20μm, the particle size of Cu powder is 5-15μm; the particle size of Mg powder is 15-10μm; the particle size of Zn powder is 5-10μm;

[0031] S2: taking 10% of the volume of the alloy powder in step S1 and drying the carbon black; the particle size of the carbon black is 3-5 μm;

[0032] S3: taking tungsten carbide powder according to 2% of the volume of the alloy powder in step S1, taking B4C powder according to 20% of the volume of the alloy powder in step S1, mixing the alloy powder, carbon black, tungsten carbide powder and B4C powder, and then ball milling under the protection of argon; the particle size of B4C powder is 5-10μm; the particle size of tungsten carbide powder is 0.5-1.5μm;

[0033] During ball milling, zirconium oxide (d = 10 mm) was used as the ball milling medium, the ball-to-material ratio was 5:1, and the ball milling speed was less than 100 r / min;

[0034] S4: The ball-milled powder is subjected to cold isostatic pressing to form an ingot, and the ingot is subjected to vacuum hot isostatic pressing to form an ingot.

[0035] The pressure of cold isostatic pressing in this step is 190-220MPa, and the holding time is 45-60min; the temperature of hot isostatic pressing is 500-580°C, the pressure is 100-150MPa, and the holding time is 2-4h.

[0036] Embodiment 3: A method for preparing a B4C reinforced aluminum-based composite material, comprising the following steps:

[0037] S1: Al-Zn-Mg-Cu alloy powder is prepared by atomizing Al powder, Zn powder, Mg powder and Cu powder; the contents of the Al powder, Zn powder, Mg powder and Cu powder are: 92.5wt% of Al powder, 5wt% of Zn powder, 1.5wt% of Mg powder and 1wt% of Cu powder respectively;

[0038] The particle size of Al powder is 10-20μm, the particle size of Cu powder is 5-15μm; the particle size of Mg powder is 15-10μm; the particle size of Zn powder is 5-10μm;

[0039] S2: taking 15% of the volume of the alloy powder in step S1 and drying the carbon black; the particle size of the carbon black is 3-5 μm;

[0040] S3: taking tungsten carbide powder according to 2% of the volume of the alloy powder in step S1, taking B4C powder according to 30% of the volume of the alloy powder in step S1, mixing the alloy powder, carbon black, tungsten carbide powder and B4C powder, and then ball milling under the protection of argon; the particle size of B4C powder is 5-10μm; the particle size of tungsten carbide powder is 0.5-1.5μm;

[0041] During ball milling, zirconium oxide (d = 10 mm) is used as the ball milling medium, the ball-to-material ratio is 5:1, and the ball milling speed is less than 100 r / min:

[0042] S4: The ball-milled powder is subjected to cold isostatic pressing to form an ingot, and the ingot is subjected to vacuum hot isostatic pressing to form an ingot.

[0043] The pressure of cold isostatic pressing in this step is 190-220MPa, and the holding time is 45-60min; the temperature of hot isostatic pressing is 500-580°C, the pressure is 100-150MPa, and the holding time is 2-4h.

[0044] Embodiment 4: A method for preparing a B4C reinforced aluminum-based composite material, comprising the following steps:

[0045] S1: Al-Zn-Mg-Cu alloy powder is prepared by atomizing Al powder, Zn powder, Mg powder and Cu powder; the contents of the Al powder, Zn powder, Mg powder and Cu powder are: 92.5wt% of Al powder, 5wt% of Zn powder, 1.5wt% of Mg powder and 1wt% of Cu powder respectively;

[0046] The particle size of Al powder is 10-20μm, the particle size of Cu powder is 5-15μm; the particle size of Mg powder is 15-10μm; the particle size of Zn powder is 5-10μm;

[0047] S2: taking 20% ​​of the volume of the alloy powder in step S1 and drying the carbon black; the particle size of the carbon black is 3-5 μm;

[0048] S3: taking tungsten carbide powder according to 2% of the volume of the alloy powder in step S1, taking B4C powder according to 15% of the volume of the alloy powder in step S1, mixing the alloy powder, carbon black, tungsten carbide powder and B4C powder, and then ball milling under the protection of argon; the particle size of B4C powder is 5-10μm; the particle size of tungsten carbide powder is 0.5-1.5μm;

[0049] During ball milling, zirconium oxide (d = 10 mm) was used as the ball milling medium, the ball-to-material ratio was 5:1, and the ball milling speed was less than 100 r / min;

[0050] S4: The ball-milled powder is subjected to cold isostatic pressing to form an ingot, and the ingot is subjected to vacuum hot isostatic pressing to form an ingot.

[0051] The pressure of cold isostatic pressing in this step is 190-220MPa, and the holding time is 45-60min; the temperature of hot isostatic pressing is 500-580°C, the pressure is 100-150MPa, and the holding time is 2-4h.

[0052] Comparative Example 1: A method for preparing a B4C reinforced aluminum-based composite material, comprising the following steps:

[0053] S1: Al-Zn-Mg-Cu alloy powder is prepared by atomizing Al powder, Zn powder, Mg powder and Cu powder; the contents of the Al powder, Zn powder, Mg powder and Cu powder are: 92.5wt% of Al powder, 5wt% of Zn powder, 1.5wt% of Mg powder and 1wt% of Cu powder respectively;

[0054] The particle size of Al powder is 10-20μm, the particle size of Cu powder is 5-15μm; the particle size of Mg powder is 15-10μm; the particle size of Zn powder is 5-10μm;

[0055] S2: taking tungsten carbide powder according to 2% of the volume of the alloy powder in step S1, taking B4C powder according to 15% of the volume of the alloy powder in step S1, mixing the alloy powder, tungsten carbide powder and B4C powder, and then ball milling under the protection of argon; the particle size of B4C powder is 5-10μm; the particle size of tungsten carbide powder is 0.5-1.5μm;

[0056] During ball milling, zirconium oxide (d = 10 mm) was used as the ball milling medium, the ball-to-material ratio was 5:1, and the ball milling speed was less than 100 r / min;

[0057] S3: The ball-milled powder is subjected to cold isostatic pressing to form an ingot, and the ingot is subjected to vacuum hot isostatic pressing.

[0058] The pressure of cold isostatic pressing in this step is 190-220MPa, and the holding time is 45-60min; the temperature of hot isostatic pressing is 500-580°C, the pressure is 100-150MPa, and the holding time is 2-4h.

[0059] The friction coefficient and wear rate of the aluminum-based composite materials prepared in the above examples and their comparative examples were tested. It can be clearly seen that the friction coefficient and wear rate of Examples 1 to 4 are significantly lower than those of Comparative Example 1, among which Example 3 has the lowest wear rate, which is 9.74×10 -5 , there is no significant difference in friction coefficient and wear rate between Example 3 and Example 4.

[0060] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a B4C reinforced aluminum-based composite material, characterized in that: It includes the following steps: S1: Al-Zn-Mg-Cu alloy powder is prepared by atomizing Al powder, Zn powder, Mg powder and Cu powder; the contents of the Al powder, Zn powder, Mg powder and Cu powder are: 85-97wt% of Al powder, 4-5wt% of Zn powder, 1-2wt% of Mg powder and 0.5-1.5wt% of Cu powder respectively; S2: taking carbon black and drying it; S3: taking tungsten carbide powder and B4C powder, mixing alloy powder, carbon black, tungsten carbide powder and B4C powder, and ball milling under the protection of argon gas; S4: The ball-milled powder is subjected to cold isostatic pressing to form an ingot, and the ingot is subjected to vacuum hot isostatic pressing to form an ingot.

2. The method for preparing a B4C reinforced aluminum-based composite material according to claim 1, characterized in that: The amount of carbon black in step S2 is 5-15% of the volume of the alloy powder in step S1.

3. The method for preparing a B4C reinforced aluminum-based composite material according to claim 1, characterized in that: The amount of tungsten carbide powder in step S3 is 1-5% of the volume of the alloy powder in step S1.

4. The method for preparing a B4C reinforced aluminum-based composite material according to claim 1, characterized in that: The amount of B4C powder in step S3 is 10-35% of the volume of the alloy powder in step S1.

5. The method for preparing a B4C reinforced aluminum-based composite material according to claim 1, characterized in that: In step S3, zirconium oxide is used as the ball milling medium, the ball-to-material ratio is (2-5):1, and the ball milling speed is lower than 100 r / min.

6. The method for preparing a B4C reinforced aluminum-based composite material according to claim 1, characterized in that: The cold isostatic pressing pressure in step S4 is 190-220 MPa, and the holding time is 45-60 min.