Polycrystalline diamond compact and preparation method thereof
Through the aging treatment of the plating bonding agent and cemented carbide matrix, the problems of uneven mixing and surface oxidation in the polycrystalline diamond composite sheet are solved, the growth and bonding strength of the diamond are improved, and the wear resistance of the product is significantly improved.
Patent Information
- Application Number
- CN202410988456.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing preparation methods for polycrystalline diamond composite sheets, the problems of uneven mixing of diamond powder and cobalt powder, surface oxidation and unsolid bonding affect product quality.
Diamond micropowder is treated by plating binder, combined with cemented carbide matrix for aging treatment and surface purification. Through vacuum reduction presintering and high-temperature sintering processes, the diamond and bonding agent are ensured uniform contact and bonding between the diamond and the binder.
It effectively improves the growth between diamonds, avoids excessive binding agents, improves the wear resistance and bonding strength of the product, and the wear ratio reaches ≥400,000.
Smart Images

Figure CN118932233A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of superhard material manufacturing, and in particular relates to a polycrystalline diamond composite sheet. The present invention also relates to a method for preparing the polycrystalline diamond composite sheet. Background Art
[0002] The common method for preparing polycrystalline diamond composite sheets is to wet-mix multi-size diamond micropowder and metal cobalt powder for a long time to prepare mixed micropowder, and then sinter the mixed powder and cemented carbide matrix together under high temperature and high pressure to prepare polycrystalline diamond composite sheets. The disadvantages of this method are that metal cobalt powder is prone to agglomeration and uneven distribution in the mixed powder during the mixing process, a large number of other impurities are introduced into the wet mixing, and the surface of diamond powder and cobalt powder is oxidized, and the bonding is not strong during the sintering process with the cemented carbide matrix. The above problems have a great impact on product quality. Summary of the invention
[0003] The purpose of the present invention is to provide a polycrystalline diamond composite sheet, which solves the problems of uneven mixing and easy oxidation of the surfaces of diamond powder and cobalt powder in the prior art.
[0004] Another object of the present invention is to provide a method for preparing the above-mentioned polycrystalline diamond compact.
[0005] The first technical solution adopted by the present invention is that the polycrystalline diamond composite sheet includes a cemented carbide substrate and a polycrystalline diamond layer. The polycrystalline diamond layer contains diamond powder and a binder raw material. According to the mass percentage, the diamond powder accounts for 80-95% and the binder raw material accounts for 5-20%.
[0006] The second technical solution adopted by the present invention is a method for preparing a polycrystalline diamond composite sheet, and the specific steps are as follows:
[0007] S1: selecting raw materials containing diamond micropowder and metal binder cobalt powder, purifying the diamond micropowder in the raw materials, and drying to obtain purified diamond micropowder;
[0008] S2: dividing the purified diamond micropowder into coarse-grained diamond micropowder and medium-fine-grained diamond micropowder, and performing incremental processing on the coarse-grained diamond micropowder to obtain plated coarse-grained diamond micropowder;
[0009] S3: Select a cemented carbide with a grade of YG10-YG11 for matrix aging treatment, then soak it in 30-60% hydrochloric acid for 10-30 seconds, then wash it with clean water until it is neutral, then soak it in alcohol for 5-30 seconds, then take it out and dry it to obtain a cemented carbide matrix;
[0010] S4: mixing the plated coarse-grained diamond powder and the medium-fine-grained diamond powder to obtain a mixed powder;
[0011] S5: assembling the mixed micro powder and the cemented carbide matrix into an assembly, and placing the assembly in a vacuum furnace for reduction pre-sintering treatment to obtain a pre-treated assembly;
[0012] S6: sintering the pretreated assembly at high temperature to obtain a polycrystalline diamond composite sheet, wherein the polycrystalline diamond layer includes a cemented carbide substrate and a polycrystalline diamond layer, and the polycrystalline diamond layer contains diamond powder and a binder raw material. In terms of mass percentage, the diamond powder accounts for 80-95% and the binder raw material accounts for 5-20%.
[0013] The present invention is also characterized in that:
[0014] The raw materials selected in S1 include, by mass percentage, 80-95% of diamond micropowder; 5-20% of metal binder cobalt powder, and a particle size of the cobalt powder is less than or equal to 1 um;
[0015] The proportion of coarse-grained diamond powder in diamond powder is greater than that of medium-fine-grained diamond powder.
[0016] In S1, the surface purification treatment of diamond micropowders of different particle sizes is specifically as follows: the mixed diamond micropowder is placed in a 60% to 80% concentration boric acid solution, heated to 500° C. to 800° C., boiled for 10 h to 20 h, then washed with high-purity water, and dried in a vacuum drying oven after washing.
[0017] The specific process of incremental processing in S2 is:
[0018] S2.1. Prepare a mixed solution of sodium hypophosphite solution and cobalt sulfate solution in a ratio of 6:2-3, wherein the concentration of the sodium hypophosphite solution is 10%-20%, and the concentration of the cobalt sulfate solution is 3%-10%;
[0019] S2.2, put the coarse diamond powder into the mixed solution obtained in S2.1 and shake for 1 to 2 hours, the mass percentage of the coarse diamond powder to the mixed solution is 1:20 to 50, and the plated coarse diamond powder is obtained.
[0020] The aging treatment process of the cemented carbide substrate in S3 is: placing the cemented carbide in a vacuum sintering furnace, sintering at 150-350°C for 20-40h, and cooling to room temperature along with the furnace.
[0021] In S4, the plated coarse-grained diamond powder and the unplated diamond powder of other particle sizes are put into an ultrasonic mixer and mixed evenly. According to the mass percentage, the plated coarse-grained diamond powder accounts for 60% to 80%, and the unplated diamond powder of other particle sizes accounts for 20% to 40%. The ultrasonic high-speed mixing process has an ultrasonic frequency of 60 to 80 Hz and an ultrasonic time of 3 to 10 minutes.
[0022] The specific method of assembling the assembly in S5 is: spreading the mixed micro powder in a metal cup, pressing the cemented carbide substrate dried in S3 on it, and assembling it into a combination of diamond powder and cemented carbide; the metal cup is any high temperature resistant metal such as molybdenum, niobium and tantalum.
[0023] The vacuum reduction pre-sintering process in S5 is: pre-sintering in a vacuum furnace, vacuumizing the furnace to a pressure of 5×10 -2 Pa, the temperature rises to 900-1000℃, and keeps warm for 3-5min; continue to evacuate until the pressure in the furnace is 3×10 -4 Pa, fill with hydrogen to reduce the assembly for 10 min, then stop; evacuate the furnace until the pressure in the furnace is 3×10 -4 Pa, continue to fill in hydrogen for reduction, and repeat this 5 to 10 times.
[0024] The S6 medium and high temperature sintering process is: sintering temperature is 1350-1500°C, pressure is 5.0-8.0GPa, and sintering time is 10-30min.
[0025] The beneficial effects of the present invention are:
[0026] (1) The preparation method of the present invention utilizes a plating binder to ensure the contact area between diamond and catalyst, thereby eliminating the phenomenon of metal binder enrichment and effectively improving the growth between diamonds;
[0027] (2) The preparation method of the present invention utilizes the highest content of coarse diamond powder to be plated and fine diamond powder to be unplated for dry mixing, which better ensures the bonding between diamonds. Fine particles can grow well between coarse particles, and there will be no excessive binder at the contact surface, thus eliminating the metal cobalt oxidation caused by wet mixing.
[0028] (3) The preparation method of the present invention simultaneously performs aging treatment and surface purification on cemented carbide, which can increase the bonding degree of the bonding surface. During the sintering process, the mixed powder is more easily grown together with the cemented carbide matrix by infiltrating the bonding surface with cobalt, and at the same time, the influence of cemented carbide stress on the performance of the produced product is reduced;
[0029] (4) The product prepared by the preparation method of the present invention is subjected to grinding and polishing processing, and the finished product is subjected to performance testing, and the wear ratio is ≥ 400,000. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a metallographic structure uniformity diagram observed by scanning electron microscope in Example 1 of the preparation method of the present invention;
[0031] Figure 2 It is a C scan internal structure diagram of the preparation method example 1 of the present invention;
[0032] Figure 3 This is a metallographic structure uniformity diagram observed by scanning electron microscope in Example 2 of the preparation method of the present invention;
[0033] Figure 4 It is a C scan internal structure diagram of Example 2 of the preparation method of the present invention;
[0034] Figure 5 This is a metallographic structure uniformity diagram observed by scanning electron microscope in Example 3 of the preparation method of the present invention;
[0035] Figure 6 This is a metallographic structure uniformity diagram observed by scanning electron microscope for a comparative example of the preparation method of the present invention. DETAILED DESCRIPTION
[0036] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0037] The polycrystalline diamond composite sheet of the present invention comprises a cemented carbide substrate and a polycrystalline diamond layer, wherein the polycrystalline diamond layer comprises diamond powder and a binder raw material, wherein the diamond powder accounts for 80-95% by mass and the binder accounts for 5-20% by mass. The thickness of the cemented carbide is 2.5-3.5 mm.
[0038] The preparation method of the above-mentioned polycrystalline diamond composite sheet is as follows:
[0039] S1: Select raw materials containing diamond micropowder and metal binder cobalt powder, purify the diamond micropowder in the raw materials, and dry to obtain purified diamond micropowder; the selected raw materials include, by mass percentage, 80-95% of diamond micropowder content; 5-20% of metal binder cobalt powder content, and the particle size of cobalt powder is less than or equal to 1um; the proportion of coarse-grained diamond micropowder in the diamond micropowder is greater than the content of other particle size diamond micropowders.
[0040] The surface purification treatment of diamond micropowders of different particle sizes is specifically as follows: the mixed diamond micropowder is placed in a 60% to 80% concentration boric acid solution, heated to 500° C. to 800° C., boiled for 10 h to 20 h, then repeatedly washed with high-purity water, and placed in a vacuum drying oven for drying after cleaning.
[0041] S2: dividing the purified diamond micropowder into coarse-grained diamond micropowder and medium-fine-grained diamond micropowder (including medium-grained diamond micropowder and fine-grained diamond micropowder, see the embodiment), and performing incremental treatment on the coarse-grained diamond micropowder to obtain plated coarse-grained diamond micropowder;
[0042] Among them, the specific process of incremental processing is:
[0043] S2.1. Prepare a mixed solution of sodium hypophosphite solution and cobalt sulfate solution in a ratio of 6:2-3, wherein the concentration of the sodium hypophosphite solution is 10%-20%, and the concentration of the cobalt sulfate solution is 3%-10%;
[0044] S2.2, put the coarse diamond powder into the mixed solution obtained in S2.1 and shake for 1 to 2 hours, the mass percentage of the coarse diamond powder to the mixed solution is 1:20 to 50, and the plated coarse diamond powder is obtained.
[0045] Chemical plating is used, and the reducing effect of sodium hypophosphite in the chemical cobalt plating solution is utilized to reduce the cobalt ions into metallic cobalt, which is deposited layer by layer. The oscillation principle is used to ensure uniform plating. The weight of metallic cobalt that needs to be increased by plating on the surface of the diamond micropowder with the highest content is calculated by weight. The cobalt purity is ≥99.9%.
[0046] S3: Select a cemented carbide with a grade of YG10-YG11 for matrix aging treatment, then immerse it in 30-60% hydrochloric acid for 10-30 seconds for purification, wash it with clean water until it is neutral, immerse it in alcohol for 5-30 seconds, then take it out and dry it to obtain a cemented carbide matrix;
[0047] The matrix aging treatment process is: placing the cemented carbide in a vacuum sintering furnace, sintering at 150-350°C for 20-40 hours, and then cooling to room temperature with the furnace.
[0048] S4: mixing the coated coarse-grained diamond powder and the uncoated medium-fine-grained diamond powder to obtain a mixed powder;
[0049] Specifically, the plated coarse-grained diamond powder and the unplated diamond powder of other particle sizes are put into an ultrasonic mixer and mixed evenly. Calculated by mass percentage, the plated coarse-grained diamond powder accounts for 60% to 80%, and the unplated diamond powder of other particle sizes accounts for 20% to 40%. The ultrasonic high-speed mixing process has an ultrasonic frequency of 60 to 80 Hz and an ultrasonic time of 3 to 10 minutes.
[0050] S5: assembling the mixed micro powder and the cemented carbide matrix into an assembly, and performing reduction pre-sintering treatment in a vacuum furnace to obtain a pre-treated assembly;
[0051] The specific method of assembling the combination is: spreading the mixed micro powder in a metal cup, pressing the cemented carbide matrix dried in S3 on it, and assembling it into a combination of diamond powder and cemented carbide; the metal cup is a high temperature resistant metal such as molybdenum, niobium, and tantalum.
[0052] The vacuum reduction pre-sintering process is as follows: the pre-sintering process is performed in a vacuum furnace, and the pressure in the furnace is 5×10 -2Pa, the temperature rises to 900-1000℃, and keeps warm for 3-5min; continue to evacuate until the pressure in the furnace is 3×10 -4 Pa, fill with hydrogen to reduce the assembly for 10 min, then stop; evacuate the furnace until the pressure in the furnace is 3×10 -4 Pa, continue to fill in hydrogen for reduction, and repeat this 5 to 10 times.
[0053] S6: sintering the pretreated assembly at high temperature to obtain the above-mentioned polycrystalline diamond composite sheet.
[0054] Among them, the high temperature sintering process is: sintering temperature is 1350-1500°C, pressure is 5.0-8.0GPa, and sintering time is 10-30min.
[0055] Example 1
[0056] The polycrystalline diamond composite sheet prepared in this embodiment includes a cemented carbide substrate and a polycrystalline diamond layer arranged on the cemented carbide substrate. The diamond and binder raw material components contained in the polycrystalline diamond layer are: 95% diamond powder and 5% binder; the diamond powder is composed of powders with three particle size distributions of 2-4μm, 5-10μm, and 8-12μm, wherein the particle size of 2-4μm accounts for 5% of the total amount of diamond powder, the particle size of 5-10μm accounts for 25% of the total amount of diamond powder, and the particle size of 8-12μm accounts for 70% of the total amount of diamond powder; the particle size of the binder Co powder is less than or equal to 1um.
[0057] A method for preparing a polycrystalline diamond composite sheet comprises the following steps:
[0058] 1) Place the mixed diamond powder into a 60% boric acid solution, heat to 600°C, boil for 10 hours, then repeatedly wash with high-purity water, dry, and purify the surface of the powder;
[0059] 2) For the diamond powder with the highest mixed particle size content of 8-12um, metal cobalt is plated according to the weight ratio by chemical plating:
[0060] A mixed solution of sodium hypophosphite solution and cobalt sulfate solution is prepared in a ratio of 6:2, wherein the concentration of the sodium hypophosphite solution is 10% and the concentration of the cobalt sulfate solution is 8%;
[0061] The coarse diamond powder was placed in the mixed solution obtained above and shaken for 1 hour, the mass percentage of the coarse diamond powder to the mixed solution was 1:20, and the plated coarse diamond powder was obtained.
[0062] 3) The cemented carbide substrate is placed in a vacuum sintering furnace, the temperature is raised to 300°C, the temperature is maintained for 30 hours, and the furnace is cooled to room temperature; the cemented carbide is then placed in a 50% hydrochloric acid aqueous solution to remove the surface oxide layer for 10 seconds, rinsed with alcohol, and dried to purify the surface of the cemented carbide;
[0063] 4) 8-12um cobalt-coated diamond powder and uncoated diamond powder of other particle sizes are prepared in a weight ratio of 6:4, and put into an ultrasonic mixer for mixing. The ultrasonic high-speed mixing process is an ultrasonic frequency of 60 Hz and an ultrasonic time of 5 minutes.
[0064] 5) The evenly mixed micro powder can be spread flat in a metal cup using a homemade scraper device, and the prepared cemented carbide matrix is pressed on top to assemble a combination of diamond powder and cemented carbide; the metal cup is molybdenum.
[0065] 6) Place the assembly into a vacuum furnace and evacuate the furnace to a pressure of 5×10 -2 Pa, the temperature was raised to 900℃ and kept for 5min; vacuum was continued until the pressure in the furnace was 3×10 -4 Pa, fill with hydrogen to reduce the assembly for 10 min, then stop; evacuate the furnace until the pressure in the furnace is 3×10 -4 Pa, continue to fill with hydrogen for reduction; repeat this process 6 times; perform vacuum reduction purification treatment;
[0066] 7) The purified assembly is sintered under high temperature and high pressure, with a sintering temperature of 1450° C., a pressure of 5.5 GPa, and a sintering time of 15 min to prepare a polycrystalline diamond composite sheet blank.
[0067] The diamond composite sheet prepared in this embodiment has good microstructure uniformity, and the bonding between diamonds is very strong. Figure 1 As shown in the figure, the polycrystalline diamond layer and cemented carbide are firmly bonded without delamination or pitting. Figure 2 shown.
[0068] Wear resistance test was carried out according to standard JB / T3235-2013. After testing: the wear ratio is 430,000, which has excellent wear resistance.
[0069] Example 2
[0070] The polycrystalline diamond composite sheet prepared in this embodiment includes a cemented carbide substrate and a polycrystalline diamond layer arranged on the cemented carbide substrate. The diamond and binder raw material components contained in the polycrystalline diamond layer are: 90% diamond powder and 10% binder; the diamond powder is composed of two kinds of particle size distributions of 1-3μm and 22-36μm, wherein the particle size of 1-3μm accounts for 25% of the total amount of diamond powder, and the particle size of 22-36μm accounts for 75% of the total amount of diamond powder; the particle size of the binder Co powder is ≤1um.
[0071] The present invention provides a method for preparing a polycrystalline diamond composite sheet, comprising the following steps:
[0072] 1) Place the mixed diamond powder into 80% boric acid solution, heat to 500°C, boil for 20 hours, then repeatedly wash with high-purity water, dry, and purify the surface of the powder;
[0073] 2) The diamond powder with the highest content of 22-36um in the mixed particle size is plated with metal cobalt according to the weight ratio by chemical plating:
[0074] A mixed solution of sodium hypophosphite solution and cobalt sulfate solution is prepared in a ratio of 6:3, wherein the concentration of the sodium hypophosphite solution is 20% and the concentration of the cobalt sulfate solution is 10%;
[0075] The coarse diamond powder was placed in the mixed solution obtained above and shaken for 2 hours, the mass percentage of the coarse diamond powder to the mixed solution was 1:40, and the plated coarse diamond powder was obtained.
[0076] 3) The cemented carbide substrate is placed in a vacuum sintering furnace, the temperature is raised to 150°C, the temperature is maintained for 40 hours, and the furnace is cooled to room temperature; the cemented carbide is then placed in a 30% hydrochloric acid aqueous solution for 30 seconds to remove the surface oxide layer, and then rinsed with alcohol and dried to purify the surface of the cemented carbide;
[0077] 4) 22-36um cobalt-coated diamond powder and uncoated diamond powder of other particle sizes are prepared in a weight percentage of 8:2, and put into an ultrasonic mixer for mixing. The ultrasonic high-speed mixing process is an ultrasonic frequency of 80 Hz and an ultrasonic time of 3 minutes;
[0078] 5) The evenly mixed micro powder can be spread flat in a metal cup using a homemade scraper device, and the prepared cemented carbide matrix is pressed on top to assemble a combination of diamond powder and cemented carbide; the metal cup is tantalum.
[0079] 6) Place the assembly into a vacuum furnace and evacuate the furnace to a pressure of 5×10 -2 Pa, the temperature was raised to 1000℃ and kept for 3min; vacuum was continued until the pressure in the furnace was 3×10-4 Pa, fill with hydrogen to reduce the assembly for 10 min, then stop; evacuate the furnace until the pressure in the furnace is 3×10 -4 Pa, continue to fill with hydrogen for reduction; repeat this process 5 times; perform vacuum reduction purification treatment;
[0080] 7) The purified assembly is sintered under high temperature and high pressure at a sintering temperature of 1350° C., a pressure of 5 GPa, and a sintering time of 10 min to prepare a polycrystalline diamond composite sheet blank.
[0081] The diamond composite sheet prepared in this embodiment has good microstructure uniformity, and the bonding between diamonds is very strong. Figure 3 As shown in the figure. The polycrystalline diamond layer and cemented carbide are firmly bonded without delamination or pitting. Figure 4 shown.
[0082] Wear resistance test was carried out according to standard JB / T3235-2013. After testing: the wear ratio is 460,000, which has excellent wear resistance.
[0083] Example 3
[0084] The polycrystalline diamond composite sheet prepared in this embodiment includes a cemented carbide substrate and a polycrystalline diamond layer arranged on the cemented carbide substrate. The diamond and binder raw material components contained in the polycrystalline diamond layer are: 94% diamond powder and 6% binder; the diamond powder is composed of powders with three particle size distributions of 2-4μm, 5-10μm, and 8-12μm, among which the particle size of 2-4μm accounts for 5% of the total amount of diamond powder, the particle size of 5-10μm accounts for 30% of the total amount of diamond powder, and the particle size of 8-12μm accounts for 65% of the total amount of diamond powder; the particle size of the binder Co powder is less than or equal to 1um.
[0085] A method for preparing a polycrystalline diamond composite sheet comprises the following steps:
[0086] 1) Place the mixed diamond powder into a 70% boric acid solution, heat to 550°C, boil for 15 hours, then repeatedly wash with high-purity water, dry, and purify the surface of the powder;
[0087] 2) The diamond powder with the highest mixed particle size content of 8-12um is plated with metal cobalt according to the weight ratio by chemical plating:
[0088] A mixed solution of sodium hypophosphite solution and cobalt sulfate solution is prepared in a ratio of 6:3, wherein the concentration of the sodium hypophosphite solution is 15% and the concentration of the cobalt sulfate solution is 3%;
[0089] The coarse diamond powder was placed in the mixed solution obtained above and shaken for 1.5 hours, the mass percentage of the coarse diamond powder to the mixed solution was 1:50, and the plated coarse diamond powder was obtained.
[0090] 3) The cemented carbide substrate is placed in a vacuum sintering furnace, the temperature is raised to 350°C, kept at this temperature for 20 hours, and cooled to room temperature along with the furnace; the cemented carbide is then placed in a 60% hydrochloric acid aqueous solution for 20 seconds to remove the surface oxide layer, rinsed with alcohol, and dried to purify the surface of the cemented carbide;
[0091] 4) 8-12um cobalt-coated diamond powder and uncoated diamond powder of other particle sizes are prepared in a weight percentage of 7:3, and put into an ultrasonic mixer for mixing. The ultrasonic high-speed mixing process is an ultrasonic frequency of 70 Hz and an ultrasonic time of 10 minutes.
[0092] 5) The uniformly mixed micro powder can be spread flat in a metal cup using a homemade scraper device, and the prepared cemented carbide matrix is pressed on top to assemble a combination of diamond powder and cemented carbide; the metal cup is niobium.
[0093] 6) Place the assembly into a vacuum furnace and evacuate the furnace to a pressure of 5×10 -2 Pa, the temperature was raised to 950℃ and kept for 4 min; vacuum was continued until the pressure in the furnace was 3×10 -4 Pa, fill with hydrogen to reduce the assembly for 10 min, then stop; evacuate the furnace until the pressure in the furnace is 3×10 -4 Pa, continue to fill with hydrogen for reduction; repeat this process 10 times; perform vacuum reduction purification treatment;
[0094] 7) The purified assembly is sintered under high temperature and high pressure, with a sintering temperature of 1500° C., a pressure of 8 GPa, and a sintering time of 30 min to prepare a polycrystalline diamond composite sheet blank.
[0095] The diamond composite sheet prepared in this embodiment has good microstructure uniformity, and the bonding between diamonds is very strong. Figure 5 shown.
[0096] Wear resistance test was carried out according to standard JB / T3235-2013. After testing: the wear ratio is 450,000, which has excellent wear resistance.
[0097] Comparative Example
[0098] The polycrystalline diamond composite sheet prepared in this embodiment includes a cemented carbide substrate and a polycrystalline diamond layer arranged on the cemented carbide substrate. The diamond and binder raw material components contained in the polycrystalline diamond layer are: 95% diamond powder and 5% binder; the diamond powder is composed of powders with three particle size distributions of 2-4μm, 5-10μm, and 8-12μm, wherein the particle size of 2-4μm accounts for 5% of the total amount of diamond powder, the particle size of 5-10μm accounts for 25% of the total amount of diamond powder, and the particle size of 8-12μm accounts for 70% of the total amount of diamond powder; the particle size of the binder Co powder is ≤1um.
[0099] The present invention provides a method for preparing a polycrystalline diamond composite sheet, comprising the following steps:
[0100] 1) Weigh a certain amount of mixed diamond powder and metal binder cobalt powder by weight.
[0101] 2) The mixed powder is put into a three-dimensional mixer for mixing, and at the same time, 20% anhydrous ethanol is added to the mixed micro powder and the mixing is continued for 24 hours.
[0102] 3) Place the mixed micro powder in a dryer and dry under vacuum.
[0103] 5) The uniformly mixed micro powder can be spread flat in a metal cup using a homemade scraper device, and the prepared cemented carbide matrix is pressed on top to assemble a combination of diamond powder and cemented carbide;
[0104] 6) Place the assembly into a vacuum furnace and evacuate the furnace to a pressure of 5×10 -2 Pa, the temperature was raised to 900℃ and kept for 5min; vacuum was continued until the pressure in the furnace was 3×10 -4 Pa, fill with hydrogen to reduce the assembly for 10 min, then stop; evacuate the furnace until the pressure in the furnace is 3×10 -4 Pa, continue to fill with hydrogen for reduction; repeat this 6 times; and perform vacuum reduction purification treatment.
[0105] 5) The purified assembly is sintered under high temperature and high pressure, with a sintering temperature of 1450° C., a pressure of 5.5 GPa, and a sintering time of 15 min to prepare a polycrystalline diamond composite sheet blank.
[0106] The microstructure of the diamond composite sheet obtained in this embodiment is observed to show that the metal binder is partially aggregated, and the bonding between diamonds has some pores, and the bonding is not sufficient. Figure 6 shown.
[0107] The wear resistance test was carried out according to the standard JB / T3235-2013. After testing: the wear ratio was 260,000, which was lower than the wear resistance of Example 1.
Claims
1. Polycrystalline diamond composite sheet, It is characterized in that It comprises a cemented carbide matrix and a polycrystalline diamond layer, wherein the polycrystalline diamond layer contains diamond micropowder and a binder raw material, wherein the diamond micropowder accounts for 80-95% by mass, and the binder raw material accounts for 5-20% by mass.
2. Preparation method of polycrystalline diamond composite sheet, It is characterized in that The specific steps are as follows: S1: selecting raw materials containing diamond micropowder and metal binder cobalt powder, purifying the diamond micropowder in the raw materials, and drying to obtain purified diamond micropowder; S2: dividing the purified diamond micropowder into coarse-grained diamond micropowder and medium-fine-grained diamond micropowder, and performing incremental processing on the coarse-grained diamond micropowder to obtain plated coarse-grained diamond micropowder; S3: Select a cemented carbide with a grade of YG10-YG11 for matrix aging treatment, then soak it in 30-60% hydrochloric acid for 10-30 seconds, then wash it with clean water until it is neutral, then soak it in alcohol for 5-30 seconds, then take it out and dry it to obtain a cemented carbide matrix; S4: mixing the plated coarse-grained diamond powder and the medium-fine-grained diamond powder to obtain a mixed powder; S5: assembling the mixed micro powder and the cemented carbide matrix into an assembly, and placing the assembly in a vacuum furnace for reduction pre-sintering treatment to obtain a pre-treated assembly; S6: sintering the pretreated assembly at high temperature to obtain a polycrystalline diamond composite sheet, wherein the polycrystalline diamond layer comprises a cemented carbide substrate and a polycrystalline diamond layer, and the polycrystalline diamond layer comprises diamond powder and a binder raw material, wherein the diamond powder accounts for 80-95% by mass and the binder raw material accounts for 5-20% by mass.
3. The method for preparing the polycrystalline diamond compact according to claim 2, It is characterized in that The raw materials selected in S1 include, by mass percentage, 80-95% of diamond powder and 5-20% of metal binder cobalt powder, wherein the particle size of the cobalt powder is less than or equal to 1 um; The proportion of coarse-grained diamond powder in the diamond powder is greater than that of medium-fine-grained diamond powder.
4. The method for preparing the polycrystalline diamond compact according to claim 2, It is characterized in that The surface purification treatment of diamond micropowders of different particle sizes in S1 is specifically as follows: the mixed diamond micropowder is placed in a 60% to 80% concentration boric acid solution, heated to 500° C. to 800° C., boiled for 10 h to 20 h, then washed with high-purity water, and dried in a vacuum drying oven after washing.
5. The method for preparing the polycrystalline diamond compact according to claim 4, It is characterized in that The specific process of the incremental processing in S2 is: S2.1, prepare a mixed solution of sodium hypophosphite solution and cobalt sulfate solution in a ratio of 6:2-3, wherein the concentration of the sodium hypophosphite solution is 10%-20%, and the concentration of the cobalt sulfate solution is 3%-10%; S2.2, placing the coarse diamond powder into the mixed solution obtained in S2.1 and shaking for 1 to 2 hours, wherein the mass percentage of the coarse diamond powder to the mixed solution is 1:20 to 50, to obtain the plated coarse diamond powder.
6. The method for preparing the polycrystalline diamond compact according to claim 2, It is characterized in that The aging treatment process of the cemented carbide substrate in S3 is as follows: placing the cemented carbide in a vacuum sintering furnace, sintering at 150-350° C. for 20-40 hours, and cooling to room temperature along with the furnace.
7. The method for preparing the polycrystalline diamond compact according to claim 2, It is characterized in that In S4, the plated coarse-grained diamond powder and the unplated diamond powder of other particle sizes are put into an ultrasonic mixer and mixed evenly. According to the mass percentage, the plated coarse-grained diamond powder accounts for 60% to 80%, and the unplated diamond powder of other particle sizes accounts for 20% to 40%. The ultrasonic high-speed mixing process has an ultrasonic frequency of 60 to 80 Hz and an ultrasonic time of 3 to 10 minutes.
8. The method for preparing the polycrystalline diamond compact according to claim 2, It is characterized in that The specific method of assembling the assembly in S5 is: spreading the mixed micro powder in a metal cup, pressing the hard alloy substrate dried in S3 onto it, and assembling a combination of diamond powder and hard alloy; the metal cup is any high temperature resistant metal such as molybdenum, niobium and tantalum.
9. The method for preparing the polycrystalline diamond compact according to claim 2, It is characterized in that The vacuum reduction pre-sintering process in S5 is: pre-sintering in a vacuum furnace, vacuumizing the furnace to a pressure of 5×10 -2 Pa, the temperature rises to 900-1000℃, and keeps warm for 3-5min; continue to evacuate until the pressure in the furnace is 3×10 -4 Pa, fill with hydrogen to reduce the assembly for 10 min, then stop; evacuate the furnace until the pressure in the furnace is 3×10 -4 Pa, continue to fill in hydrogen for reduction, and repeat this 5 to 10 times.
10. The method for preparing the polycrystalline diamond compact according to claim 2, It is characterized in that The S6 medium-high temperature sintering process is as follows: the sintering temperature is 1350-1500° C., the pressure is 5.0-8.0 GPa, and the sintering time is 10-30 min.