Eutectic high-entropy alloy, preparation method and application thereof and heat-treatment-free laser additive repairing method for metal parts

Through eutectic high-entropy alloy and laser additive manufacturing technology, the damage problem of heat treatment to matrix performance in the repair of high-temperature alloy parts is solved, and efficient and high-performance repair is achieved under heat-free conditions, forming nano-layered eutectic structures, taking into account both High temperature strength and thermal stability.

CN118932236AActive Publication Date: 2024-11-12TIANMUSHAN LABORATORY +1

Patent Information

Application Number
CN202411015233.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

During the repair process of high-temperature alloy components, heat treatment is required to regulate the precipitation phase and grain, resulting in a decline in matrix performance. It is difficult to take into account the high-temperature strength, thermal stability and additive manufacturing applicability of eutectic alloys.

Method used

Eutectic high entropy alloy Co20-24%, Al 9-11%, Fe 20-24%, Hf0.5-5%, Y 0.005-1%, C 0.005-1%, B0.005-1%, Ni The remaining materials are prepared by aerosolization treatment, combined with laser additive manufacturing technology, and realize efficient and high-performance repair of metal parts under heat-free treatment. The multi-main high entropy effect and high Hf, C and other reinforcement designs are used. A nano-layered eutectic two-phase structure is formed.

Benefits of technology

It realizes efficient and high-performance repair of metal parts, avoids secondary damage to the performance of substrate materials by heat treatment after traditional additive repair, has mechanical properties comparable to high-temperature alloys, and does not require additional heat treatment. It is suitable for high-efficiency and high-efficiency and high-temperature alloy parts. Performance repair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932236A_ABST
    Figure CN118932236A_ABST
Patent Text Reader

Abstract

The invention provides a eutectic high-entropy alloy, a preparation method and application thereof and a heat-treatment-free laser additive repairing method for metal parts, and belongs to the technical field of alloy materials. The eutectic high-entropy alloy disclosed by the invention comprises the following elements: 20 to 24 percent of Co, 9 to 11 percent of Al, 20 to 24 percent of Fe, 0.5 to 5 percent of Hf, 0.005 to 1 percent of Y, 0.005 to 1 percent of C, 0.005 to 1 percent of B and the balance of Ni. The eutectic high-entropy alloy has better thermal stability by utilizing a multi-principal-element high-entropy effect and high-Hf, C and other strengthening design, the eutectic high-entropy alloy is used as a repairing material, and a laser additive manufacturing technology is utilized, so that the obtained repairing material has a nano layered eutectic two-phase structure, has the mechanical property equivalent to that of a high-temperature alloy without heat treatment, and is suitable for the repair of the high-temperature alloy. The problem of secondary damage of heat treatment after traditional additive repair to the performance of a base material is solved, and the method is suitable for efficient and high-performance repair of high-temperature alloy metal parts sensitive to the heat process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alloy materials, and in particular to a eutectic high entropy alloy, a preparation method and application thereof, and a heat treatment-free laser additive repair method for metal parts. Background Art

[0002] During the service of hot-end high-temperature alloy parts in aerospace power, energy and chemical industries, some key parts will have cracks and other defects due to deformation, wear, corrosion and other reasons, which will have serious negative impacts on the safety and efficiency of the equipment. These parts have high performance requirements and are generally expensive. If the surface damage can be effectively repaired, and its performance can be restored and improved, it can effectively ensure the normal operation of the equipment, reduce production costs, and achieve significant economic benefits.

[0003] Laser additive repair is an advanced remanufacturing technology that uses a high-power laser beam as an energy source to repair locally damaged parts. This technology has the characteristics of high repair accuracy, high efficiency, small heat-affected zone, small workpiece damage, good microstructure and performance in the repaired area, and high material utilization. Since it can be formed to near-size, it has obvious technical advantages in ensuring the geometric dimensional accuracy of repairing waste products or parts, and is one of the feasible technologies for repairing hot-end high-temperature alloy parts.

[0004] However, the high temperature strength of high temperature alloys is often achieved by solid phase transformation precipitation strengthening phase. Therefore, the use of high temperature alloy powder for repair technology requires heat treatment to achieve the tempering and performance goals. On the other hand, the heat treatment process will also have an adverse effect on the repair object. At present, alloy materials used for parts repair usually need to be heat treated to carry out precipitation phase and grain regulation to achieve performance optimization and improvement. Taking GH4169 alloy as an example, the laser additive GH4169 repair layer is mainly composed of columnar dendrites and equiaxed dendrites. There is obvious element segregation behavior between dendrites, mainly enriched with Nb and Mo, and poor in Fe, Cr and Ni. The repair layer is mainly composed of matrix γ phase, Laves phase, MC carbide and MN nitride. It must be treated with high temperature solid solution and aging to effectively refine the grains and eliminate the Laves segregation phase, thereby effectively improving the mechanical properties of the repair layer. However, the repaired workpiece matrix has already undergone a solid solution and aging heat treatment during the preparation process of the workpiece matrix. Heat treatment with the repair layer again will cause the growth of the matrix grains and significantly reduce the matrix performance.

[0005] Eutectic alloy is a material with eutectic precipitation as the main strengthening mechanism, that is, a two-phase structure directly formed during solidification that generally does not require heat treatment to regulate and optimize, producing precipitation and interface strengthening effects. However, this type of material generally has difficulty in balancing high-temperature strength, high-temperature thermal stability and applicability for additive manufacturing. Summary of the invention

[0006] The purpose of the present invention is to provide a eutectic high entropy alloy, a preparation method and application, and a laser additive repair method for metal parts without heat treatment. The eutectic high entropy alloy provided by the present invention is used in the laser additive repair of metal parts, and a better repair effect can be guaranteed without heat treatment.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The invention provides a eutectic high entropy alloy, which comprises, by mass percentage, the following elements: Co20-24%, Al 9-11%, Fe 20-24%, Hf0.5-5%, Y 0.005-1%, C 0.005-1%, B0.005-1%, and Ni balance.

[0009] The present invention provides a method for preparing the eutectic high entropy alloy described in the above technical solution, comprising the following steps:

[0010] The raw materials are prepared according to the elemental composition of the eutectic high entropy alloy and then smelted, and the obtained alloy liquid is gas-atomized to obtain the eutectic high entropy alloy.

[0011] Preferably, the smelting is carried out at a vacuum degree of 5×10 -3 ~1×10 -4 MPa conditions;

[0012] The conditions of the atomization treatment include: the protective gas used is an inert gas, the diameter of the nozzle used is 4 mm, the atomization pressure is 4-10 MPa, and the atomization treatment time is 5-15 min.

[0013] The present invention provides the use of the eutectic high entropy alloy described in the above technical solution or the eutectic high entropy alloy prepared by the preparation method described in the above technical solution in heat treatment-free laser additive repair of metal parts.

[0014] Preferably, the material of the metal component is a high-temperature alloy; the laser additive repair method includes laser selective melting forming repair or laser coaxial powder feeding repair.

[0015] The present invention provides a laser additive repair method for metal parts without heat treatment, comprising the following steps:

[0016] The eutectic high entropy alloy described in the above technical solution or the eutectic high entropy alloy prepared by the preparation method described in the above technical solution is used as a repair material to perform laser additive repair on the metal parts to be repaired.

[0017] Preferably, the material of the metal parts to be repaired is a high-temperature alloy; the laser additive repair method includes laser selective melting forming repair or laser coaxial powder feeding repair.

[0018] Preferably, the conditions for the laser selective melting forming repair include: the particle size of the eutectic high entropy alloy used is 15-53 μm; the laser power is 215-335 W, the scanning rate is 800-1100 mm / s, the powder layer thickness is 30-60 μm, and the scanning interval is 80-120 μm; the scanning method is a strip scanning method, and each layer is rotated 67° after completion of the scan.

[0019] Preferably, the conditions for the laser coaxial powder feeding repair include: the particle size of the eutectic high entropy alloy used is 53-150 μm; the laser power is 1800-2200 W, the scanning rate is 720-960 mm / s, the powder feeding amount is 12-14 g / min, the overlap width is 1-1.6 mm, and the spot diameter is 0.5-3 mm; the interlayer residence time is 30-60 s.

[0020] Preferably, after the laser additive repair is completed, a repair material is directly obtained without heat treatment, and the repair material has a nano-layered eutectic two-phase structure.

[0021] Beneficial effects: The present invention utilizes the composition design and thermal stability of eutectic high entropy alloy, the construction of additive manufacturing microstructure and low defective process, and the process optimization for heat-free treatment, to provide a eutectic high entropy alloy and preparation method and a heat-free laser additive repair method for metal parts, solving the problem of high-efficiency and high-performance heat-free repair of metal parts. Specifically, the present invention provides a eutectic high entropy alloy, the element composition of which includes, by mass percentage: Co 20-24%, Al 9-11%, Fe 20-24%, Hf0.5-5%, Y 0.005-1%, C 0.005-1%, B 0.005-1%, and Ni balance. The present invention controls the proportion of main elements and the content of trace elements such as Hf, utilizes the high entropy effect of multiple main elements and strengthening designs such as high Hf and C, and can make the eutectic high entropy alloy have good thermal stability. It is used as a repair material and uses laser additive manufacturing technology to successfully repair metal parts without heat treatment. The obtained repair material has a nano-layered eutectic two-phase structure and has mechanical properties equivalent to those of high-temperature alloys without additional heat treatment. It solves the problem of secondary damage to the performance of the matrix material caused by heat treatment after traditional additive repair, and is suitable for efficient and high-performance repair of high-temperature alloy metal parts that are sensitive to thermal processes.

[0022] Specifically, the eutectic high entropy alloy provided by the present invention utilizes the high entropy and dual-phase synergistic strengthening and toughening mechanism to replace the traditional alloy solid phase reaction precipitation strengthening, and at the same time utilizes the strong thermal gradient and high cooling rate non-equilibrium processing conditions of laser additive manufacturing technology to prepare a nano-layered structure, and combines fine grain strengthening to achieve performance compatibility and heat treatment-free performance. Wherein the eutectic high entropy alloy described in the present invention utilizes microstructure regulation without adding precious metal elements, that is, the unique ultrafine dual-phase lamellar structure of the eutectic high entropy alloy, and the soft and hard phases have the strength and plasticity advantages of both face-centered cubic and body-centered cubic high entropy alloys, and with the increase of service time and service temperature, there is no initiation of new phases in the organization and significant degradation of the lamellar dual phase. The room temperature tensile strength of the printed state of the eutectic high entropy alloy is significantly better than that of the printed state of GH4169, and the printed state of the eutectic high entropy alloy can achieve the room temperature mechanical performance level of the standard heat treatment state of GH4169 forgings without heat treatment, realizing low-cost and low-density substitution under the same service conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a SEM image of the alloy powder with a particle size of 15 to 53 μm prepared in Example 1;

[0024] Figure 2 These are photos of printed samples 1-10 in Example 2;

[0025] Figure 3 The SEM images of the printed samples 1-10 in Example 2;

[0026] Figure 4 is the room temperature tensile stress-strain curve of printed samples 1-10 in Example 2;

[0027] Figure 5 This is a schematic diagram of the sample tissue observation plane;

[0028] Figure 6 SEM images of printed samples 1-10;

[0029] Figure 7 The SEM images of printed samples 1-10 treated at 600°C for 6 hours;

[0030] Figure 8 The SEM images of printed samples 1-10 treated at 700°C for 6 hours;

[0031] Fig. 9 The SEM images of printed samples 1-10 treated at 800°C for 6 hours;

[0032] Fig.10 The SEM images of printed samples 1-10 treated at 900°C for 6 hours;

[0033] Fig.11 The SEM images of printed samples 1-10 treated at 1000°C for 6 hours;

[0034] Fig.12 The SEM images of printed samples 1-10 treated at 1300℃ for 2h;

[0035] Fig.13 This is a photo of the repaired sample in Example 3;

[0036] Fig.14 This is the SEM image of the repaired sample in Example 3. DETAILED DESCRIPTION

[0037] The invention provides a eutectic high entropy alloy, which comprises, by mass percentage, the following elements: Co20-24%, Al 9-11%, Fe 20-24%, Hf0.5-5%, Y 0.005-1%, C 0.005-1%, B0.005-1%, and Ni balance.

[0038] The element composition of the eutectic high entropy alloy provided by the present invention includes, by mass percentage: Co 20-24%, specifically 20%, 21%, 22%, 23% or 24%; Al 9-11%, specifically 9%, 9.5%, 10%, 10.5% or 11%; Fe 20-24%, specifically 20%, 21%, 22%, 23% or 24%; Hf0.5-5%, specifically 0.5%, 1%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%; Y0.005-1%, specifically 0.005%, 0.01%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5% or 1%; C 0.005-1%, specifically 0.005%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%; B 0.005-1%, specifically 0.005%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%; and Ni balance. The present invention controls each element in the eutectic high entropy alloy (wherein C, B, and Hf are grain boundary strengthening elements) within the above range, and uses the eutectic high entropy alloy in the laser additive repair of metal parts, which can ensure a good repair effect without heat treatment. In the present invention, the eutectic high entropy alloy is specifically a powder material, and the particle size of the eutectic high entropy alloy is preferably 15 to 150 μm (specifically 15 to 53 μm or 53 to 150 μm). In the actual application process, the eutectic high entropy alloy of the required particle size can be obtained by screening according to the specific process requirements. The present invention can make the eutectic high entropy alloy have good thermal stability by controlling the proportion of the main elements and the content of trace elements such as Hf. It is used as a repair material and uses laser additive manufacturing technology to achieve successful repair of metal parts without heat treatment.

[0039] The present invention provides a method for preparing the eutectic high entropy alloy described in the above technical solution, comprising the following steps:

[0040] The raw materials are prepared according to the elemental composition of the eutectic high entropy alloy and then smelted, and the obtained alloy liquid is gas-atomized to obtain the eutectic high entropy alloy.

[0041] The present invention prepares raw materials according to the elemental composition of the eutectic high entropy alloy and then smelts them to obtain a molten alloy. The present invention has no special restrictions on the raw materials for preparation. Raw materials (such as alloys) familiar to those skilled in the art can be used as long as the elemental composition of the final product meets the above requirements. In the present invention, the smelting is preferably carried out under a vacuum degree of 5×10 -3 ~1×10 -4 MPa; the vacuum degree is more preferably 6×10 -3 MPa. In the present invention, the smelting is preferably carried out in a smelting furnace.

[0042] After obtaining the alloy liquid, the present invention performs atomization treatment on the alloy liquid to obtain the eutectic high entropy alloy. In the present invention, the conditions of the atomization treatment include: the protective gas used is preferably an inert gas, the inert gas is preferably argon, and the purity of the argon is preferably 99.9%; the diameter of the nozzle used is preferably 4mm, and the nozzle is preferably a graphite nozzle; the aerosol pressure is preferably 4-10MPa, more preferably 8MPa; the aerosol treatment time is preferably 5-15min, more preferably 12min. The present invention preferably sprays the alloy liquid into an atomization tower through a nozzle, and performs the atomization treatment in the presence of an inert gas; the alloy liquid is crushed by an inert gas by adjusting the aerosol pressure and cooled to obtain a powdered eutectic high entropy alloy.

[0043] After the aerosol treatment, the present invention preferably performs screening according to specific process requirements to obtain a eutectic high entropy alloy of a desired particle size; the equipment used for the screening is preferably a powder sieving machine.

[0044] The present invention provides the use of the eutectic high entropy alloy described in the above technical solution or the eutectic high entropy alloy prepared by the preparation method described in the above technical solution in the laser additive repair of metal parts without heat treatment. In the present invention, the material of the metal parts is preferably a high-temperature alloy, and the high-temperature alloy preferably includes a nickel-based high-temperature alloy or a high-entropy alloy; the laser additive repair method preferably includes laser selective melting forming repair or laser coaxial powder feeding repair.

[0045] The present invention innovatively applies the eutectic precipitation theory, that is, a two-phase structure can be formed from the time of solidification, or a two-phase structure and possible precipitation and interface strengthening effects can be provided in a heat-free state. Since the repair target object is a high-temperature alloy, the repair material needs to have high-temperature strength, so the high-entropy thermal strengthening effect is selected, combined with the eutectic behavior, the eutectic high-entropy alloy and additive manufacturing are cleverly used to solve the problem of repairing high-temperature alloy parts. It depends on creative work in the design of eutectic high-entropy alloy composition and thermal stability, additive manufacturing microstructure construction and low-defect process, and process optimization for heat-free treatment. Specifically, the powdered eutectic high-entropy alloy provided by the present invention is used as a repair material, and both the laser selective melting forming repair process and the laser coaxial powder feeding repair process can form samples without macro cracks and with high density. The present invention cleverly utilizes comprehensive means such as the high entropy effect of multiple main elements, the in-situ generation of dual-phase structure by eutectic, and the production of nano-layered structure by laser additive manufacturing. Through the coordination of composition and process, a "one-step manufacturing" material repair technology with multi-scale construction of "atomic stability-microstructure-mesostructure" has been developed. The performance is equivalent to that of classic high-temperature alloys such as GH4169 without heat treatment. The feature of no heat treatment solves the problem of secondary damage to the performance of the matrix material due to heat treatment after repair additive manufacturing. It is suitable for the efficient and high-performance repair of high-temperature alloy metal parts that are sensitive to the heat treatment process, and the implementation process conditions are relatively simple, suitable for popularization and application.

[0046] The present invention provides a laser additive repair method for metal parts without heat treatment, comprising the following steps:

[0047] The eutectic high entropy alloy described in the above technical solution or the eutectic high entropy alloy prepared by the preparation method described in the above technical solution is used as a repair material to perform laser additive repair on the metal parts to be repaired.

[0048] In the present invention, the material of the metal parts to be repaired is preferably a high-temperature alloy, and the high-temperature alloy preferably includes a nickel-based high-temperature alloy or a high-entropy alloy; the laser additive repair method preferably includes laser selective melting forming repair or laser coaxial powder feeding repair, which is described in detail below.

[0049] In the present invention, the substrate used for the laser selective melting forming repair is preferably a 304 stainless steel substrate; the present invention preferably preheats the substrate before performing the laser selective melting forming repair, and the preheating temperature is preferably 80-130°C, more preferably 95°C. In the present invention, the substrate is preferably surface treated before preheating, and the surface treatment preferably includes: sandblasting the upper surface of the substrate with a sandblaster in advance, washing with acetone to remove surface debris, and then washing with alcohol and drying.

[0050] In the present invention, the eutectic high entropy alloy used for laser selective melting forming repair is dried before use, and the drying is preferably carried out under vacuum conditions; the drying temperature is preferably 120-150°C, more preferably 130°C; the drying time is preferably 1-3h, more preferably 2h.

[0051] In the present invention, the conditions for the laser selective melting forming repair include: the particle size of the eutectic high entropy alloy used is preferably 15-53 μm; the laser power is preferably 215-335 W, preferably 245-305 W, and more preferably 275 W; the scanning rate is preferably 800-1100 mm / s, and more preferably 900-1000 mm / s; the thickness of the powder layer is preferably 30-60 μm, and more preferably 40 μm; the scanning spacing is preferably 80-120 μm, and more preferably 100 μm; the scanning mode is a strip scanning mode, and each layer is rotated 67° after scanning to ensure that the scanning direction will be completely repeated after processing multiple layers, thereby reducing the accumulation of residual stress. The present invention preferably optimizes the laser selective melting forming repair under the above conditions, which is conducive to improving the compactness of the eutectic high entropy alloy, while reducing the residual stress inside the eutectic high entropy alloy, avoiding the formation of cracks in the alloy, and the obtained eutectic high entropy alloy has good mechanical properties without subsequent treatment (such as heat treatment).

[0052] In the present invention, the laser selective melting forming repair is preferably carried out in a protective atmosphere, the protective atmosphere is preferably argon, and the purity of the argon is preferably ≥99.99%; the oxygen content in the protective atmosphere is preferably <400ppm, more preferably <350ppm. The present invention preferably carries out the laser selective melting forming repair in a protective atmosphere, which can prevent the powdered eutectic high entropy alloy from undergoing an oxidation reaction with oxygen in the air.

[0053] The present invention uses laser selective melting technology to rapidly process and form eutectic high entropy alloys using a focused laser beam to obtain nearly dense components. At the same time, the ultra-fast cooling rate can prevent the formation of brittle intermetallic compounds and element segregation to a certain extent, thereby obtaining eutectic high entropy alloy components with refined structure and uniform composition. On the other hand, the laser selective melting technology is not constrained by the complex shape of the formed part, and parts with complex shapes and high surface accuracy can be obtained, which effectively improves production efficiency, reduces production costs, and broadens the application field of eutectic high entropy alloys.

[0054] In the present invention, the eutectic high entropy alloy used for laser coaxial powder feeding repair is dried before use, and the drying is preferably carried out under vacuum conditions; the drying temperature is preferably 120-150°C, more preferably 130°C; the drying time is preferably 1-3h, more preferably 2h.

[0055] In an embodiment of the present invention, the metal parts to be repaired used in the laser coaxial powder feeding repair are DD432 single crystal alloy cylinders that have undergone standard heat treatment. The cylinder diameter is 15 mm. The cross-section is pre-polished with sandpaper to a bright mirror surface, then cleaned with ethanol and blown dry. Finally, the metal parts to be repaired are placed securely on the forming platform.

[0056] In the present invention, the conditions for the laser coaxial powder feeding repair include: the particle size of the eutectic high entropy alloy used is preferably 53-150 μm; the laser power is preferably 1800-2200 W, more preferably 2000 W; the scanning rate is preferably 720-960 mm / s, more preferably 840 mm / s; the powder feeding amount is preferably 12-14 g / min, more preferably 13.3 g / min; the overlap width is preferably 1-1.6 mm, more preferably 1.4 mm; the spot diameter is preferably 0.5-3 mm, more preferably 2 mm; the interlayer residence time is preferably 30-60 s, more preferably 40 s. The present invention chooses to add an interlayer residence, which is beneficial to ensure that each layer of cladding repair has a better effect. The present invention preferably performs laser coaxial powder feeding repair under the above conditions, which is beneficial to improving the density of the eutectic high entropy alloy, while reducing the residual stress inside the eutectic high entropy alloy, avoiding the formation of cracks in the alloy, and enhancing the interface bonding strength between the matrix (i.e., the metal parts to be repaired) and the repaired part. The interface bonding effect is good, and the obtained repaired parts (i.e., the repaired metal parts) do not need to be subsequently processed (such as heat treatment) to have good mechanical properties.

[0057] In the present invention, the laser coaxial powder feeding repair is preferably carried out in a protective atmosphere, the protective atmosphere is preferably argon, and the purity of the argon is preferably ≥99.99%; the oxygen content in the protective atmosphere is preferably <400ppm, more preferably <350ppm. The present invention preferably carries out the laser coaxial powder feeding repair in a protective atmosphere to achieve epitaxial growth, which can prevent the powdered eutectic high entropy alloy from undergoing an oxidation reaction with oxygen in the air.

[0058] In the present invention, after the laser additive repair is completed, a repair material is directly obtained without heat treatment, and the repair material has a nano-layered eutectic two-phase structure.

[0059] In the present invention, the high entropy alloy is different from the design principle of traditional alloys, and has a multi-principal high entropy effect. Although there are many principal elements, a solid solution structure is formed, which has mechanical properties such as high hardness, high wear resistance and high strength that are superior to traditional alloys. Moreover, through the reasonable compounding of elements, a eutectic high entropy alloy can be designed to generate a two-phase structure in situ, thereby having both a face-centered cubic with excellent plasticity and a body-centered cubic with high strength, and achieving an excellent match between strength and plasticity. At the same time, advanced laser additive processes can utilize non-equilibrium processing conditions of strong thermal gradients and high cooling rates to prepare nano-layered structures, greatly improving the two-phase synergistic strengthening effect of eutectic high entropy alloys. Combining the above effects, the eutectic high entropy alloy provided by the present invention can generate a multi-phase structure of nano-sheets through a eutectic reaction during the solidification process, and does not need to be precipitated through a heat treatment solid phase change to achieve two-phase / multi-phase regulation. The eutectic high entropy alloy provided by the present invention is used in the laser additive repair of metal parts, and a good repair effect can be guaranteed without heat treatment.

[0060] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] Example 1

[0062] In terms of mass percentage, the composition of the eutectic high entropy alloy in this embodiment is as follows: Co 23%, Al 10%, Fe 22%, Hf 2%, Y 0.1%, C 0.5%, B 0.5%, and Ni balance;

[0063] The mixed raw materials were placed in a melting furnace according to the composition of the eutectic high entropy alloy and vacuumed to 6×10 -3 MPa, smelting is carried out to obtain alloy liquid;

[0064] The alloy liquid is sprayed into an atomizing tower using a graphite nozzle with a diameter of 4 mm, and argon gas with a purity of 99.9% is filled as a protective gas. The atomization is performed for 12 minutes under the condition of an atomization pressure of 8 MPa. During the atomization process, the alloy liquid is crushed by argon gas and cooled to obtain alloy powder;

[0065] The alloy powder is sieved by a powder sieving machine to obtain alloy powder with a particle size of 15 to 53 μm (subsequently used for laser selective melting forming repair process) and alloy powder with a particle size of 53 to 150 μm (subsequently used for laser coaxial powder feeding repair process).

[0066] Figure 1This is a SEM image of the alloy powder with a particle size of 15 to 53 μm prepared in Example 1. The results show that the particle size of the alloy powder is uniform.

[0067] Example 2

[0068] The alloy powder with a particle size of 15 to 53 μm prepared in Example 1 was used as a eutectic high entropy alloy powder for laser additive repair without heat treatment to carry out a laser selective melting forming repair process experiment, as follows:

[0069] The alloy powder with a particle size of 15 to 53 μm prepared in Example 1 was placed in a drying oven, heated to 130° C. in a vacuum environment for drying for 2 hours, and then cooled in the oven and the obtained dry alloy powder was added to the powder feeding cylinder of the laser selective melting equipment;

[0070] The forming substrate is 304 stainless steel. The upper surface of the forming substrate is sandblasted in advance with a sandblasting machine, and cleaned with acetone to remove surface debris, then cleaned with ethanol and blown dry. The dried forming substrate is installed on the forming platform and leveled, and then preheated to 95°C;

[0071] Turn on the laser selective melting forming equipment and set the printing parameters: laser power, scanning speed, scanning spacing and powder layer thickness are specifically shown in Table 1; laser selective melting forming repair is carried out in a closed chamber under the protection of high-purity argon (argon purity ≥99.99%, oxygen content <350ppm), wherein the scanning mode is a strip scanning mode, and after completing each layer of scanning, it is rotated 67° to obtain a eutectic high entropy alloy printed sample.

[0072] Table 1 SLM process parameters

[0073]

[0074] According to Table 1, the optimal process parameters are as follows: laser power 275W, scanning speed 1000mm / s, scanning spacing 0.1mm, and powder layer thickness 0.04mm. The photos of the printed samples of eutectic high entropy alloys (referred to as printed samples 1-10) prepared under the optimal process parameters are shown in Figure 1. Figure 2 shown.

[0075] The microstructure observation and mechanical property test of printed samples 1-10 are as follows:

[0076] Figure 3 This is the SEM image of the printed sample 1-10 in Example 2. The results show that the microstructure of the printed sample 1-10 is an extremely fine and dense two-phase eutectic structure (the density of the printed sample 1-10 is >99%).

[0077] Figure 4The room temperature tensile stress-strain curve of the printed sample 1-10 in Example 2, the mechanical properties comparison data of the printed sample 1-10 and the GH4169 printed state and the GH4169 forging standard heat treatment state are shown in Table 2. The results show that the room temperature tensile mechanical properties of the printed sample 1-10 provided by the present invention are excellent, significantly better than the room temperature tensile mechanical properties of the GH4169 printed state, and can reach the room temperature tensile mechanical properties of the GH4169 forging standard heat treatment state without heat treatment.

[0078] Table 2 Mechanical properties of printed samples 1-10, GH4169 printed samples, and GH4169 forgings in standard heat treatment state

[0079]

[0080] The printed samples 1-10 were heat-treated at 600° C., 700° C., 800° C., 900° C., 1000° C. for 6 h and at 1300° C. for 2 h, respectively, and the microstructure changes were observed, as follows:

[0081] Figure 5 This is a schematic diagram of the sample tissue observation plane, and the observed tissue is a plane perpendicular to the printing direction.

[0082] Figure 6 These are SEM images of printed samples 1-10, where most of the longitudinal sections of rod-shaped tissue can be observed in the left-hand organization diagram, while the cross-sections of rod-shaped tissue can be observed in the right-hand organization diagram. The results show that the BCC phase is a fishbone-shaped short rod tissue.

[0083] Figure 7 These are SEM images of printed samples 1-10 treated at 600°C for 6 hours. In the left-hand microstructure diagram, most of the longitudinal sections are rod-shaped structures, while in the right-hand microstructure diagram, the cross-sections are rod-shaped structures. The results show that a few rod-shaped BCCs are connected.

[0084] Figure 8 These are SEM images of printed samples 1-10 treated at 700°C for 6 hours. In the left-hand organizational diagram, most of the longitudinal sections are rod-shaped tissues, while in the right-hand organizational diagram, the cross-sections are rod-shaped tissues. The results show that most of the rod-shaped BCCs are connected to form lamellar tissues.

[0085] Fig. 9 These are SEM images of printed samples 1-10 treated at 800°C for 6 hours. In the left-hand microstructure diagram, it can be observed that most of them are longitudinal sections of lamellar tissue, while in the right-hand microstructure diagram, they are cross-sections of lamellar tissue. The results show that all the rod-like BCC phases are connected to form lamellar tissue.

[0086] Fig.10This is the SEM image of printed samples 1-10 after heat treatment at 900℃ for 6h. The results show that the BCC layers are connected to form a maze-like layer structure.

[0087] Fig.11 The SEM images of printed samples 1-10 treated at 1000℃ for 6h show that the BCC layers are interconnected and grow.

[0088] Fig.12 This is the SEM image of printed samples 1-10 after heat treatment at 1300℃ for 2h. The results show that at high temperature, the two-phase lamellae are merged into large lamellae, and the two phases are still stable.

[0089] Depend on Figure 6 to Figure 12 It can be seen that the eutectic high entropy alloy provided by the present invention has good organizational stability and overheat resistance. As the service temperature increases, there is no initiation of new phases in the organization and significant degradation of the lamellar dual phase.

[0090] Example 3

[0091] The alloy powder with a particle size of 53 to 150 μm prepared in Example 1 was used as a eutectic high entropy alloy powder for laser additive repair without heat treatment to carry out a laser coaxial powder feeding repair process experiment, as follows:

[0092] The alloy powder with a particle size of 53 to 150 μm prepared in Example 1 was placed in a drying oven, heated to 130° C. in a vacuum environment for drying for 2 h, and then cooled in the oven and the obtained dry alloy powder was added to the powder feeding cylinder of the laser coaxial powder feeding device;

[0093] The metal parts to be repaired are DD432 single crystal alloy cylinders that have undergone standard heat treatment. The cylinder diameter is 15 mm. The cross section is pre-polished with sandpaper to a bright mirror surface, then cleaned with ethanol and blown dry. The blown-dried metal parts to be repaired are placed securely on the forming platform.

[0094] Turn on the laser coaxial powder feeding equipment and set the printing parameters: spot diameter is 2mm, powder feeding amount is 13.3g / min, overlap width is 1.4mm, laser power is 2000W, scanning rate is 840mm / s, and interlayer residence time is 40s; coaxial powder feeding repair is carried out in a closed chamber under the protection of high-purity argon (argon purity ≥99.99%, oxygen content <350ppm) to obtain a repaired sample.

[0095] The repaired sample is observed with naked eyes, and the metallographic structure of the repaired interface is inspected. Fig.13 This is a photo of the repaired sample in Example 3. Fig.14 is the SEM image of the repaired sample in Example 3; Fig.13 and Fig.14It can be seen that no cracks were found in the repaired sample.

[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A eutectic high entropy alloy, characterized in that: The element composition includes, by mass percentage, Co 20-24%, Al 9-11%, Fe 20-24%, Hf 0.5-5%, Y 0.005-1%, C 0.005-1%, B 0.005-1%, and Ni balance.

2. The method for preparing the eutectic high entropy alloy according to claim 1, characterized in that: The following steps are involved: The raw materials are prepared according to the elemental composition of the eutectic high entropy alloy and then smelted, and the obtained alloy liquid is gas-atomized to obtain the eutectic high entropy alloy.

3. The preparation method according to claim 2, characterized in that: The melting temperature is 5×10 -3 ~1×10 - 4 MPa conditions; The conditions of the atomization treatment include: the protective gas used is an inert gas, the diameter of the nozzle used is 4 mm, the atomization pressure is 4-10 MPa, and the atomization treatment time is 5-15 min.

4. Application of the eutectic high entropy alloy according to claim 1 or the eutectic high entropy alloy prepared by the preparation method according to claim 2 or 3 in laser additive repair of metal parts without heat treatment.

5. The use according to claim 4, characterized in that: The material of the metal parts is a high-temperature alloy; the laser additive repair method includes laser selective melting forming repair or laser coaxial powder feeding repair.

6. A laser additive repair method for metal parts without heat treatment, comprising the following steps: The eutectic high entropy alloy described in claim 1 or the eutectic high entropy alloy prepared by the preparation method described in claim 2 or 3 is used as a repair material to perform laser additive repair on the metal parts to be repaired.

7. The method for laser additive repair of metal parts without heat treatment according to claim 6, characterized in that: The material of the metal parts to be repaired is a high-temperature alloy; the laser additive repair method includes laser selective melting forming repair or laser coaxial powder feeding repair.

8. The method for laser additive repair of metal parts without heat treatment according to claim 7, characterized in that: The conditions for the laser selective melting forming repair include: the particle size of the eutectic high entropy alloy used is 15 to 53 μm; the laser power is 215 to 335 W, the scanning rate is 800 to 1100 mm / s, the powder layer thickness is 30 to 60 μm, and the scanning spacing is 80 to 120 μm; the scanning method is a strip scanning method, and each layer is rotated 67° after completion of the scan.

9. The method for laser additive repair of metal parts without heat treatment according to claim 7, characterized in that: The conditions for the laser coaxial powder feeding repair include: the particle size of the eutectic high entropy alloy used is 53-150 μm; the laser power is 1800-2200 W, the scanning rate is 720-960 mm / s, the powder feeding amount is 12-14 g / min, the overlap width is 1-1.6 mm, the spot diameter is 0.5-3 mm; and the interlayer residence time is 30-60 s.

10. The laser additive repair method for metal parts without heat treatment according to any one of claims 6 to 9 The method is characterized in that After the laser additive repair is completed, the repair material is directly obtained without heat treatment. The repair material has a nano-layered eutectic two-phase structure.

Citation Information

Patent Citations

  • Light-weight high-entropy alloy and manufacturing process of impeller made of light-weight high-entropy alloys

    CN110396634A

  • High-nickel eutectic high-entropy alloy powder for additive manufacturing and preparation method of high-nickel eutectic high-entropy alloy powder

    CN111519078A

  • Preparation method of high-entropy alloy powder laser cladding layer

    CN112226766A

  • Double-phase high-entropy high-temperature alloy and additive manufacturing method thereof

    CN113215468A

  • Complex-shape structural part formed through additive manufacturing and containing high-entropy alloy

    CN114643362A

Cited By

  • Method for manufacturing labyrinth type regulating valve based on additive manufacturing mode

    CN119794376A

  • High-strength, high-toughness and high-entropy alloy composite material and preparation method thereof

    CN120533115A