Ti-Ca treated pressure vessel steel plate for hydrogen storage and manufacturing method of Ti-Ca treated pressure vessel steel plate
Through Ti-Ca treatment and specific process design, the mechanical properties and low-temperature toughness of the steel plate for hydrogen storage pressure vessel are improved, and the problems of the reduced mechanical properties of existing steel plates and insufficient low-temperature impact toughness in high-pressure hydrogen environment are solved, achieving high Improved strength and anti-hydrocrack properties.
Patent Information
- Application Number
- CN202410861847.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The existing pressure vessel steel plates for hydrogen storage have problems such as reduced mechanical properties and insufficient low-temperature impact toughness in high-pressure hydrogen environments, which are difficult to meet the needs of the steel industry.
The pressure vessel steel plate for hydrogen storage using Ti-Ca treatment can improve the mechanical properties of the steel plate and the toughness of the welding heat-affected zone through specific chemical composition design and two-stage control rolling process, combined with tempering heat treatment, and improve the mechanical properties of the steel plate and the toughness of the welding heat-affected zone to ensure yield strength and resistance. Tensile strength and low-temperature impact toughness.
The high strength, good low-temperature performance and anti-hydrocracking performance of the steel plate are achieved, and the steel plate manufacturing requirements for pressure vessels with a thickness of 20-50mm are met. The mechanical properties of the welding heat-affected zone are significantly improved, the low-temperature impact toughness and anti-hydrocracking performance are anti-hydrocracking performance. Achieving an excellent level.
Smart Images

Figure BDA0004919314690000091 
Figure BDA0004919314690000092 
Figure BDA0004919314690000101
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of hydrogen storage pressure vessel steel plates, and in particular to a hydrogen storage pressure vessel steel plate treated with Ti-Ca and a manufacturing method thereof, which is particularly suitable for gas hydrogen storage tanks. Background Art
[0002] Oxide metallurgy technology refers to the fact that certain types and sizes of non-metallic inclusions in steel can promote the nucleation and induced nucleation of intragranular ferrite in the coarse-grained zone of the heat-affected zone during welding. Ferrite nucleates and grows on non-metallic inclusions in the superheated austenite crystals, forming radial intragranular acicular ferrite laths that divide the austenite grains into multiple small parts, while the intragranular acicular ferrite is interlocked, and there are mostly large-angle grain boundaries between the laths, which requires more energy to be consumed during the crack propagation process, thereby effectively improving the toughness of the steel. Steel plates are usually processed and manufactured using efficient and high-energy-density welding methods, with welding heat input of more than 100kJ / cm. The one-pass welding of hydrogen storage pressure vessel steel plates can significantly reduce manufacturing costs and improve production efficiency. Therefore, it has become an urgent task for the steel industry to study hydrogen storage pressure vessel steel plates with excellent welding performance and resistance to hydrogen-induced cracking.
[0003] Hydrogen energy has the characteristics of wide sources, convenient storage and transportation, efficient utilization, clean and environmentally friendly. It is an important means to support the clean use of fossil energy and the scale of renewable energy. The compatibility of steel plates with high-pressure hydrogen is something that needs to be considered for steel plates used in pressure vessels for hydrogen storage. At room or low temperatures, it is generally believed that there is no risk of bubbling or cracking when hydrogen is stored in commonly used carbon steel materials. However, the diffusion of hydrogen in metals under high pressure can still lead to a decrease in the mechanical properties of steel, especially plasticity and toughness. In summary, it is urgent to develop a steel plate for hydrogen storage pressure vessels with excellent comprehensive performance to meet the needs of the steel industry. For example, in CN115896616A "A normalizing pressure vessel steel plate that is easy to weld and a manufacturing method", its chemical composition is: C: 0.16-0.19%, Si: 0.15-0.40%, Mn: 1.45-1.65%, P: ≤0.010%, S: 0.003-0.010%, Ni: 0.40-0.80%, and other elements. The composition of the designed pressure vessel steel plate is relatively complex, and the carbon equivalent setting range is relatively high. The steel plate is prone to welding thermal cracks, which affects the processing and manufacturing of the steel plate; CN112813353A "A super-high temperature SPWHT high-toughness normalizing container steel and a manufacturing method" optimizes the normalizing process and simulated post-weld heat treatment process by adopting reasonable proportions and rolling processes, but the low-temperature impact toughness cannot be guaranteed, and the strength of the steel plate is low after normalizing heat treatment and simulated post-weld heat treatment processes. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention aims to provide a hydrogen storage container steel plate treated with Ti-Ca and a manufacturing method thereof, through the design of the composition, the production process of the two-stage controlled rolling, and the quenching and tempering heat treatment. The mechanical properties of the steel plate of the present invention and the mechanical properties of the simulated post-weld heat treatment meet the following requirements: yield strength ReL ≥ 650MPa, tensile strength Rm: 800-920MPa, elongation A ≥ 21%, -50℃ low temperature impact toughness KV2 ≥ 100J, -50℃ low temperature tensile yield strength R eL ≥660MPa, tensile strength R m :820~930MPa, elongation ≥21%; use high wire energy 100~140kJ / cm to weld steel plates, the yield strength of the welding heat affected zone (HAZ) R eL ≥690MPa, tensile strength R m : 830~950MPa, elongation ≥17%, -50℃ welding heat affected zone (HAZ) impact toughness KV2 ≥70J. (20-50)mm thickness steel plate has excellent strength and low temperature impact toughness, and has uniform and fine structure, which can meet the manufacturing and application requirements of steel plates for pressure vessels.
[0005] The object of the invention is achieved in this way:
[0006] A steel plate for a hydrogen storage pressure vessel treated with Ti-Ca comprises the following components by weight percentage: C: 0.09% to 0.12%, Si: 0.25% to 0.40%, Mn: 1.10% to 1.30%, P: ≤0.015%, S: ≤0.005%, Cr: 0.30% to 0.40%, Ni: 0.20% to 0.30%, Mo: 0.09% to 0.18%, V: 0.09% to 0.15%, Nb: 0.01% to 0.02%, Ti: 0.01% to 0.02%, Al: 0.003% to 0.005%, Ca: 0.006% to 0.008%, V / C ≥ 1, Ti / Ca: 1 to 3. The balance is Fe and unavoidable impurities.
[0007] Furthermore, V / C≥1.
[0008] Furthermore, Ti / Ca:1~3.
[0009] Furthermore, the steel plate has a yield strength of ≥650MPa, a tensile strength of 800-950MPa, A ≥21% and a low-temperature impact toughness of -50°C ≥100J.
[0010] Furthermore, the steel microstructure is tempered bainite+acicular ferrite, the volume percentage of the tempered bainite structure is 92-96%; the grain size of the microstructure is 8-10 levels, and the average size of the composite inclusions is 2-4 μm.
[0011] Furthermore, the thickness of the steel plate is 20 to 50 mm.
[0012] In order to achieve the above object, the present invention designs a hydrogen storage container steel plate treated with Ti-Ca, and the chemical composition (by mass %) of the steel used is as follows:
[0013] C: 0.09% ~ 0.12%, Si: 0.25% ~ 0.40%, Mn: 1.10% ~ 1.30%, P: ≤ 0.015%, S: ≤ 0.005%, Cr: 0.30% ~ 0.40%, Ni: 0.20% ~ 0.30%, Mo: 0.09% ~ 0.18%, V: 0.10% ~ 0.30%, Nb: 0.01% ~ 0.02%, Ti: 0.01% ~ 0.02%, Al: 0.003% ~ 0.005%, Ca: 0.006% ~ 0.008%, V / C ≥ 1, Ti / Ca: 1 ~ 3, the balance is Fe and unavoidable impurities.
[0014] The reasons for the composition design of the present invention are as follows:
[0015] The invention reduces the Mn content in the steel on the basis of the strengthening elements of C, Si and Mn, ensures that the steel plate has sufficient strength and reduces the cost of the steel plate; in order to ensure that the steel plate has high strength, V element is added to play a fine grain strengthening effect to refine the grains, and the large-angle grain boundaries in the organization are increased, which can inhibit the extension of cracks and reduce the sensitivity of welding cracks, and the ratio of V to C is adjusted to increase the formed carbides, so that the hydrogen storage capacity and hydrogen corrosion resistance of the steel plate in a low-temperature and high-pressure service environment can be improved; the Cr element content is increased, the dissolution rate of carbides is reduced, the toughness and hardenability of the steel are improved, and the local decarburization caused by the penetration and diffusion of H atoms in the metal lattice can also be reduced. The Cr-containing carbides generated after heat treatment are dissolved in the matrix and refine the grains, thereby improving the hydrogen resistance of the steel plate; Ti element is added, and after Ti-Ca treatment, the number of composite inclusions in the organization is increased, the austenite grains are refined, and the formation of acicular ferrite is promoted, the strength and toughness of the steel plate are improved, and the mechanical properties of the welding heat affected zone (HAZ) can be improved after Ti-Ca treatment.
[0016] C: 0.09%~0.12%
[0017] C forms various carbides with alloy elements in steel to strengthen the steel. It is an element that directly improves the strength of the steel plate. Too high a C content will lead to poor toughness, plasticity and welding performance of the steel. In order to ensure that the steel plate has good low-temperature impact toughness, strength and welding performance during use, the C content is limited to 0.09% to 0.12%.
[0018] Si: 0.25%~0.40%
[0019] Si is an element that increases carbon activity in steel. In the high silicon concentration area, it can reduce the diffusion flow of carbon to carbides, inhibit the coarsening of carbides, and a certain amount of Si can increase the strength of steel plates, improve the hardenability of steel, and within a certain range can reduce the ductile-brittle transition temperature and improve the plasticity of steel. Therefore, the Si content is limited to 0.25% to 0.40%.
[0020] Mn: 1.10%~1.30%
[0021] Mn plays a role of solid solution strengthening in steel. It can be dissolved in Fe matrix in large quantities to improve the strength and hardness of steel plate, improve hot working performance, prevent hot cracks, and improve the distribution of sulfides. And the content in the range of 0.6-1.6% can improve the toughness of weld metal and the solubility of Nb and V in steel. However, if the Mn content is too high, it is easy to form segregation in the steel plate, which is not good for plasticity and toughness. Therefore, Mn is limited to 1.10%-1.30%.
[0022] P:≤0.015%
[0023] P is a harmful element in steel, which has a great impact on low temperature impact toughness and is also an element that is very easy to segregate, so its content should be controlled to be low during the steelmaking process. The present invention controls P within a range that does not affect the performance, so the P content is controlled to be below 0.015%.
[0024] S:≤0.005%
[0025] S is also a harmful element in steel. It is easy to form MnS in steel, generate defects, and easily become the source of crack formation in subsequent processing. It also has a great influence on the toughness of steel. However, considering the operability and cost of steelmaking, S is controlled below 0.005%.
[0026] Cr: 0.30%~0.40%
[0027] Cr, as the main element of this patent, is an element that stabilizes carbides. Adding chromium reduces the dissolution rate of carbides, improves the toughness and hardenability of steel, and reduces local decarburization caused by the penetration and diffusion of H atoms in the metal lattice. During the quenching and tempering process, the generated Cr23C6 type carbides are dissolved in the matrix and play a role in refining the grains. Therefore, the Cr content is controlled between 0.30% and 0.40%.
[0028] Ni: 0.20%~0.30%
[0029] Ni is the main element for stabilizing austenite in steel. Ni can exist in austenite and ferrite in the form of solid solution with Fe, so it can improve the strength of steel, refine the grains, and improve the low-temperature impact toughness of steel. However, due to the high cost of nickel, it will also make it difficult to remove the iron oxide scale of the steel plate, thereby increasing the cost, so the Ni content is limited to between 0.20% and 0.30%.
[0030] Mo: 0.09%~0.18%
[0031] Mo can reduce the austenite transformation zone in steel, promote ferrite transformation, dissolve in ferrite, austenite and carbide, improve the strength of steel plate, and after quenching and tempering treatment, it can improve the temper brittleness resistance of steel plate, reduce internal residual stress and improve the plasticity of steel plate. Therefore, the content of Mo is controlled to be between 0.09% and 0.18%.
[0032] V: 0.09%~0.15%
[0033] V can dissolve into austenite at high temperature and increase the hardenability of steel. Microalloying can promote the increase of VC, VN, V(C,N) complex compounds formed in steel, stabilize carbides, pin at grain boundaries, inhibit grain boundary movement and grain growth, and ensure the hardness of steel plates through precipitation strengthening, precipitation strengthening and fine grain strengthening, improve the strength and plasticity of steel plates, and improve the toughness and tempering stability of steel; adjust the ratio of V to C, increase the carbides formed by vanadium and carbon in steel, and improve the hydrogen storage capacity and hydrogen corrosion resistance of steel plates in low temperature and high pressure service environments. Therefore, V is limited to 0.10% to 0.30%.
[0034] Nb: 0.01%~0.02%
[0035] Nb in steel can inhibit austenite recrystallization during rolling, promote grain refinement, improve strength and toughness, reduce overheating sensitivity and temper brittleness, improve welding performance, and can also produce solid solution strengthening, precipitating a large amount of Nb (C, N) on grain boundaries and dislocations. Therefore, Nb is limited to 0.01% to 0.02%.
[0036] Ti: 0.01%~0.02%
[0037] Ti, as the main element of this patent, can form a large number of dispersed fine TiN or TiO particles. After Ti treatment during the steelmaking process, fine inclusion particles TiO can be obtained, which can promote the formation of acicular ferrite in the grains during the solidification of the structure, thereby playing a role in refining the grains; Ti (C, N) precipitated first at high temperature can promote the precipitation of Nb and V. However, when w (Ti) ≥ 0.09%, the acicular ferrite content will be reduced, and the low-temperature toughness of the steel plate will deteriorate, so the Ti content is limited to 0.01% to 0.02%.
[0038] Al: 0.003%~0.005%
[0039] Al is the main deoxidizer in steel, which can fix N elements, refine grains, and improve the toughness of steel. Adding Al before Ca treatment for full deoxidation can ensure the recovery rate of Ca in steel. Therefore, the Al content is limited to 0.003% to 0.005%.
[0040] Ca: 0.006%~0.008%
[0041] Ca acts as a deoxidizing and desulfurizing agent in steel, and can change the morphology and distribution of non-metallic inclusions. By increasing the number of inclusions, the austenite grain size can be refined. After heat treatment, the inclusions can become spheroidized and small, providing nucleation sites for acicular ferrite. It can also effectively refine and control the weld heat affected zone (HAZ) structure to improve the toughness of the weld heat affected zone. Therefore, the Ca content is limited to 0.006% to 0.008%. An appropriate amount of Ca combined with a trace amount of Ti can increase the number of inclusions to refine the austenite grains, so the Ti / Ca ratio is limited to 1 to 3.
[0042] The second technical solution of the present invention is to provide a method for manufacturing a steel plate for a hydrogen storage pressure vessel treated with Ti-Ca, comprising smelting, continuous casting, heating, rolling, cooling, and heat treatment;
[0043] The present invention provides a method for preparing a hydrogen storage pressure vessel steel plate treated with Ti-Ca, wherein the ingredients are prepared according to the chemical composition range designed by the present invention, Ti-Ca elements are used for treatment during oxygen converter smelting, the effect of oxide metallurgy is fully exerted, and after vacuum treatment, full-process protection casting is used during continuous casting, and fine composite inclusions are generated during solidification to refine the ingot grains; the finished steel plate has a thickness specification of 20 to 50 mm, and the rolling process adopts two-stage controlled rolling and controlled cooling to refine the structure and control the size and distribution of inclusions; the inclusions can inhibit the growth of austenite grains in the welding heat affected zone (HAZ) during subsequent welding, and improve the low-temperature toughness of the welding heat affected zone; after quenching and tempering heat treatment, the inclusions can become spheroidized, provide nucleation sites for acicular ferrite, and the structure is further uniform, so that the steel plate has low welding crack sensitivity. Finally, the mechanical properties and hydrogen resistance of the steel plate are tested to obtain a hydrogen storage pressure vessel steel plate.
[0044] The specific production process steps are as follows:
[0045] Smelting
[0046] The molten steel is first pre-treated in an argon station, and then Ti treatment and deoxidation are carried out, followed by deep dephosphorization and desulfurization, so that the P content in the molten iron is reduced to less than 0.015%, and the S content is reduced to less than 0.005%. Then the addition of Al is strictly controlled, and Ca treatment is carried out 10 to 20 minutes after Al deoxidation, and non-metallic inclusions are deformed; LF furnace refining is used to adjust the composition, ensuring that the argon soft blowing time is ≥12 minutes and the refining time is 30 to 60 minutes; RH vacuum treatment is used for further refining and adjustment of the composition, ensuring that the molten steel temperature is 1600 to 1630°C, and the vacuum treatment time is 40 to 80 minutes, so that the harmful inclusions in the molten steel can fully float, ensuring the purity of the molten steel and sufficient micro-alloying treatment time of the molten steel. By deforming the non-metallic inclusions in the molten steel, the role of oxide metallurgy is brought into play, the quality of the continuous casting billet is improved, and beneficial composite inclusion particles are obtained, providing a heterogeneous nucleation core for subsequent organization formation.
[0047] casting
[0048] The casting process is argon protected during the entire casting process. The casting process adopts the light pressure reduction technology, the pressure reduction is controlled at 2-5mm, and the casting speed is controlled at 1.0-1.4m / min to eliminate the internal defects of the casting and improve the surface quality of the casting. The beneficial composite inclusion particles can provide nucleation points for the grains of the casting to refine the grains of the casting. The secondary cooling water is controlled at 5000-6000L / min, and the casting superheat is 15-30℃ to improve the central segregation and central looseness of the casting and improve the internal quality of the casting. The billet straightening temperature is controlled at 950±30℃ to ensure the quality of the casting and reduce the generation of cracks in the casting, so as to obtain a continuous casting billet with a thickness of 250-360mm. Finally, the slab is cleaned, slowly cooled, and the quality of the continuous casting billet is inspected.
[0049] heating
[0050] The heating of continuous casting billet is divided into preheating section, heating section and soaking section: the preheating section is controlled at 780±30℃, the heating section is controlled at 1250~1280℃, the soaking section is controlled at 1200-1240℃, and the total time of the billet in the furnace is 210-240min; by heating the billet in three stages, the temperature of the core of the billet reaches 1180~1220℃, ensuring that the billet structure is completely austenite; but when the heating temperature is higher than 1280℃, it is easy to cause excessive growth of grains inside the billet, affecting the distribution of beneficial inclusions inside the structure.
[0051] Rolling
[0052] After the billet is out of the furnace, a two-stage controlled rolling and controlled cooling technology is adopted. First, rough rolling is carried out, the starting rolling temperature is controlled at 1130-1180℃, the rolling speed is controlled at 1.3-1.8m / s, and the single-pass reduction rate of rough rolling is controlled at 12%-18%, ensuring that the total reduction rate of rough rolling is ≥60% to fully refine the austenite grains; the starting rolling temperature of finishing rolling is 900±50℃, the rolling speed is controlled at 2.0-2.5m / s, the rolling temperature of the final rolling pass is controlled at 820-840℃, the single-pass reduction rate of finishing rolling is ≥10%, and the total reduction rate of finishing rolling is ≥55%. The grains are further flattened and elongated, and the increase in the grain boundary area provides more nucleation sites for the subsequent phase transformation process. By controlling the total reduction rate of rough rolling and finishing rolling, the grains of the steel plate are sufficiently refined and the internal defects of the steel plate are eliminated. After rolling, controlled cooling is performed, with the start cooling temperature of 740-800℃, the red-returning temperature of 560-630℃, and the cooling rate of 10-21℃ / s to ensure fine grains, promote the formation of fine precipitates, and improve the mechanical properties of the steel plate. Then the steel plate is stacked and slowly cooled, with the slow cooling temperature of 450-550℃, the number of stacks of 11-15 sheets, and the stacking time of 16-24h, so that H and O in the steel plate have enough time to be eliminated. The thickness of the obtained steel plate is 20-50mm.
[0053] Heat Treatment
[0054] The steel plate is stacked and slowly cooled before being subjected to quenching and tempering heat treatment. To ensure the various performance indicators of the steel plate, the steel plate is subjected to quenching and tempering heat treatment process, with a quenching temperature of 930±10°C, a quenching heating rate of 1.5±0.3min / mm, a tempering temperature of 610±10°C, a tempering heating rate of 1.2±0.2min / mm, and air cooling after the heat treatment. Through quenching and tempering heat treatment, the beneficial composite inclusion particles are spheroidized and fine, and the fine precipitates in the organization are evenly distributed, ensuring that the steel plate has high strength and good low-temperature performance, and the steel plate organization is uniform, the organization is tempered troostite + acicular ferrite organization, tempered troostite organization (92-96% by volume) + acicular ferrite (4-8% by volume), the grain size is 8-10, and the average size of the composite inclusions is 2-4μm.
[0055] The beneficial effects of the present invention are:
[0056] The present invention aims to develop a hydrogen storage pressure vessel steel plate with excellent comprehensive performance. An alloy composition is designed with an efficient and economical process, taking both cost and performance into consideration. Ti-Ca treatment is used in the smelting process, and fine composite inclusions are obtained through oxide metallurgy technology to refine the ingot grains to improve the quality of the continuous casting ingot. Two-stage controlled rolling and controlled cooling are used to refine the structure and control the size and distribution of inclusions. The inclusions can inhibit the growth of austenite grains in the welding heat affected zone (HAZ) during the subsequent welding process and improve the mechanical properties of the welding heat affected zone. After quenching and tempering heat treatment, the inclusions can become spheroidized, providing nucleation sites for acicular ferrite, and the structure is further uniform, so that the steel plate has low welding crack sensitivity. Finally, the mechanical properties and hydrogen resistance of the steel plate are tested to obtain a hydrogen storage pressure vessel steel plate.
[0057] 1. The microstructure of the steel plate of the present invention is uniform and fine, and the final microstructure is tempered troostite + acicular ferrite, tempered troostite structure (92-96% by volume) + acicular ferrite (4-8% by volume), the grain size is 8-10, and the average size of the composite inclusions is 2-4 μm, so that the comprehensive mechanical properties of the steel plate are excellent.
[0058] 2. The thickness of the steel plate of the present invention is 20-50 mm. After the steel plate for container is subjected to the quenching and tempering heat treatment process, the steel plate has high strength performance, good low temperature performance, and good resistance to hydrogen-induced cracking. Its mechanical properties are: yield strength ReL ≥ 650 MPa, tensile strength Rm: 800-920 MPa, elongation A ≥ 21%, -50°C low temperature impact toughness KV2 ≥ 100 J, -50°C low temperature tensile yield strength R eL ≥660MPa, tensile strength R m :820~930MPa, elongation ≥21%.
[0059] 3. The present invention uses a large line energy of 100-140 kJ / cm to weld the steel plate, and the yield strength R of the heat affected zone (HAZ) of the welding eL ≥690MPa, tensile strength R m : 830~950MPa, elongation ≥17%, -50℃ welding heat affected zone (HAZ) impact toughness KV2≥70J.
[0060] 4. The HIC resistance of the steel plate was measured in accordance with GB / T 8650-2015 "Evaluation Method for Hydrogen Induced Cracking Resistance of Pipeline Steel and Pressure Vessel Steel", and the results showed that the designed steel grade has good HIC resistance. Hydrogen induced cracking resistance: crack length percentage CLR ≤ 5%, crack thickness percentage CTR ≤ 5%, crack sensitivity percentage CSR ≤ 3%.
[0061] 5. The present invention simulates the post-weld heat treatment process to test the mechanical properties of the steel plate, the simulated post-weld heat treatment temperature is 600-640°C, and the holding time is 120-360min. Its mechanical properties are: yield strength ReL≥650MPa, tensile strength Rm: 800-920MPa, elongation A≥21%, -50°C low temperature impact toughness KV2≥100J. DETAILED DESCRIPTION
[0062] The present invention will be further described below by way of examples.
[0063] The embodiment of the present invention performs smelting, continuous casting, heating, rolling, cooling and heat treatment according to the component ratio of the technical solution, and is characterized in that:
[0064] Smelting
[0065] First, Ti treatment is used for deoxidation, then Ca treatment is carried out, and non-metallic inclusions in molten steel are deformed; LF furnace refining is used to adjust the composition, dephosphorization and desulfurization are carried out, and the argon soft blowing time is ensured to be ≥12min, and the refining time is 30-60min; then RH vacuum treatment is used for refining and adjusting the composition, and the molten steel temperature is ensured to be between 1600 and 1630℃, and the vacuum treatment time is 40-80min;
[0066] heating
[0067] The preheating section is controlled at 780±30℃, the heating section is controlled at 1250~1280℃, the soaking section is controlled at 1200-1240℃, and the total slab in the furnace time is 210-240min;
[0068] Rolling
[0069] The starting rolling temperature is controlled at 1130-1180℃, the rolling speed is controlled at 1.3-1.8m / s, and the single-pass rough rolling reduction rate is controlled at 12%-18%, ensuring that the total rough rolling reduction rate is ≥60% to fully refine the austenite grains; the starting rolling temperature of the finishing rolling is 900±50℃, the rolling speed is controlled at 2.0-2.5m / s, the final rolling temperature is controlled at 820-840℃, the roller speed is controlled at 0.5-0.7m / s, the single-pass finishing reduction rate is ≥10%, ensuring that the total finishing reduction rate is ≥55%
[0070] cool down
[0071] After rolling, the steel plate is controlled to cool, the cooling temperature is 740-800℃, the red-return temperature is 560-630℃, the cooling rate is 10-21℃ / s, and then the steel plate is stacked and slowly cooled, the slow cooling temperature is 450~550℃, the stacking quantity is 11~15 sheets, and the stacking time is guaranteed to be 16~24h;
[0072] Heat Treatment
[0073] The steel plate is first subjected to a quenching and tempering heat treatment process, with a quenching temperature of 930±10°C, a quenching heating rate of 1.5±0.3min / mm, a tempering temperature of 610±10°C, a tempering heating rate of 1.2±0.2min / mm, and air cooling after the quenching and tempering heat treatment.
[0074] Furthermore, the continuous casting process casts the billet under argon protection throughout the casting process, adopts light reduction technology to cast the billet, the reduction amount is controlled at 2-5mm, the billet drawing speed is controlled at 1.0-1.4m / min, the casting superheat is controlled at 15-30°C, and the billet straightening temperature is controlled at 950±30°C.
[0075] The embodiments specifically illustrate the content of the present invention. These embodiments are only general descriptions of the content of the present invention and do not limit the content of the present invention. Table 1 is the chemical composition of the embodiment, Table 2 is the smelting and casting method of the embodiment, Table 3 is the rolling process parameters of the embodiment, Table 4 is the cooling and heat treatment process parameters of the embodiment, Table 5 is the mechanical properties of the embodiment, Table 6 is the mechanical properties of the welding heat affected zone of the embodiment, Table 7 is the mechanical properties of the heat treatment after welding of the embodiment steel, and Table 8 is the organization, grain size and hydrogen cracking resistance test results of the embodiment.
[0076] Table 1 Chemical composition of the examples (wt%)
[0077]
[0078] Table 2 Example smelting and casting method
[0079]
[0080] Table 3 Example rolling process parameters
[0081]
[0082] Table 4 Cooling and heat treatment process parameters of the embodiment
[0083]
[0084] Table 5 Mechanical properties of the examples
[0085]
[0086] Table 6 Mechanical properties of heat affected zone of welding of example
[0087]
[0088] Table 7 Mechanical properties of example steel after heat treatment
[0089]
[0090] Table 8 Example organization, grain size and hydrogen induced cracking test results
[0091]
[0092] Samples were taken from the heat-treated steel plate for performance testing. The test was carried out in accordance with GB / T 228.3-2019 "Metallic Materials Tensile Test Part 1: Low Temperature Test Method" and GB / T 229-2020 "Metallic Materials Charpy Pendulum Impact Test Method", which shows that the steel plate has high strength and toughness, good low temperature performance, and can be used in the low temperature service environment of hydrogen storage; the grain size was measured in accordance with GB / T6394-2017 "Method for Determination of Average Grain Size of Metals", and the grain size of the steel plate was above grade 8.5, which shows that the crack sensitivity of the steel plate is low; the HIC resistance of the steel plate was measured in accordance with GB / T 8650-2015 "Evaluation Method for Hydrogen-Induced Cracking of Pipeline Steel and Pressure Vessel Steel", and the results showed that the designed steel grade has good HIC resistance.
[0093] As can be seen from the above, the container steel plate with a thickness of 20 to 50 mm of the present invention has high strength performance, good -50°C low temperature impact toughness, and good hydrogen-induced crack resistance after quenching and tempering heat treatment. Its mechanical properties are: yield strength ReL ≥ 650MPa, tensile strength Rm: 800 to 920MPa, elongation A ≥ 21%, -50°C low temperature impact toughness KV2 ≥ 100J, -50°C low temperature tensile yield strength R eL ≥660MPa, tensile strength R m:820~930MPa, elongation ≥21%; use high wire energy 100~140kJ / cm to weld steel plates, the yield strength of the welding heat affected zone (HAZ) R eL ≥690MPa, tensile strength R m : 830~950MPa, elongation ≥17%, -50℃ welding heat affected zone (HAZ) impact toughness KV2≥70J.
[0094] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A steel plate for a hydrogen storage pressure vessel treated with Ti-Ca, It is characterized in that Measured by weight percentage, it includes the following components: C: 0.09% ~ 0.12%, Si: 0.25% ~ 0.40%, Mn: 1.10% ~ 1.30%, P: ≤0.015%, S: ≤0.005%, Cr: 0.30% ~ 0.40%, Ni: 0.20% ~ 0.30%, Mo: 0.09% ~ 0.18%, V: 0.09% ~ 0.15%, Nb: 0.01% ~ 0.02%, Ti: 0.01% ~ 0.02%, Al: 0.003% ~ 0.005%, Ca: 0.006% ~ 0.008%, and the balance is Fe and unavoidable impurities.
2. The hydrogen storage pressure vessel steel plate treated with Ti-Ca according to claim 1, It is characterized in that V / C≥1.
3. The hydrogen storage pressure vessel steel plate treated with Ti-Ca according to claim 1, It is characterized in that Ti / Ca:1~3.
4. The hydrogen storage pressure vessel steel plate treated with Ti-Ca according to claim 1, It is characterized in that Yield strength ReL ≥ 650MPa, tensile strength Rm: 800 ~ 920MPa, elongation A ≥ 21%, -50℃ low temperature impact toughness KV 2 ≥100J, -50℃ low temperature tensile yield strength R eL ≥660MPa, tensile strength R m :820~930MPa, elongation ≥21%.
5. The hydrogen storage pressure vessel steel plate treated with Ti-Ca according to claim 1, It is characterized in that The steel plate is welded with a high wire energy of 100-140 kJ / cm. The yield strength of the heat affected zone (HAZ) is R eL ≥690MPa, tensile strength R m : 830~950MPa, elongation ≥17%, -50℃ welding heat affected zone (HAZ) impact toughness KV 2 ≥70J.
6. The hydrogen storage pressure vessel steel plate treated with Ti-Ca according to claim 1, It is characterized in that The steel microstructure is tempered troostite+acicular ferrite, the volume percentage of the tempered troostite is 92-96%, the microstructure grain size is 8-10, and the average size of the composite inclusions is 2-4 μm.
7. The hydrogen storage pressure vessel steel plate treated with Ti-Ca according to claim 1, It is characterized in that The thickness of the steel plate is 20 to 50 mm.
8. A method for manufacturing a hydrogen storage pressure vessel steel plate treated with Ti-Ca according to any one of claims 1 to 6, comprising smelting, continuous casting, heating, rolling, cooling, heat treatment, It is characterized in that Smelting First, Ti treatment is used for deoxidation, then Ca treatment is carried out, and non-metallic inclusions in molten steel are deformed; LF furnace refining is used to adjust the composition, dephosphorization and desulfurization are carried out, and the argon soft blowing time is ensured to be ≥12min, and the refining time is 30-60min; then RH vacuum treatment is used for refining and adjusting the composition, and the molten steel temperature is ensured to be between 1600 and 1630℃, and the vacuum treatment time is 40-80min; heating The preheating section is controlled at 780±30℃, the heating section is controlled at 1250~1280℃, the soaking section is controlled at 1200-1240℃, and the total slab in the furnace time is 210-240min; Rolling The rolling temperature is controlled at 1130-1180°C, the rolling speed is controlled at 1.3-1.8 m / s, and the rough rolling single pass reduction rate is controlled at 12%-18%, ensuring that the total rough rolling reduction rate is ≥60% to fully refine the austenite grains; The start rolling temperature of finishing rolling is 900±50℃, the rolling speed is controlled at 2.0~2.5m / s, the rolling temperature of the final rolling pass is controlled at 820~840℃, the roller speed is controlled at 0.5~0.7m / s, the single-pass reduction rate of finishing rolling is ≥10%, and the total reduction rate of finishing rolling passes is guaranteed to be ≥55%; cool down After rolling, the steel plate is controlled to cool, the cooling temperature is 740-800℃, the red-return temperature is 560-630℃, the cooling rate is 10-21℃ / s, and then the steel plate is stacked and slowly cooled, the slow cooling temperature is 450~550℃, the stacking quantity is 11~15 sheets, and the stacking time is guaranteed to be 16~24h; Heat Treatment The steel plate is first subjected to a quenching and tempering heat treatment process, with a quenching temperature of 930±10°C, a quenching heating rate of 1.5±0.3min / mm, a tempering temperature of 610±10°C, a tempering heating rate of 1.2±0.2min / mm, and air cooling after the quenching and tempering heat treatment.
9. The method for manufacturing a hydrogen storage pressure vessel steel plate treated with Ti-Ca according to claim 7, It is characterized in that The continuous casting process casts the billet under argon protection throughout the casting process, adopts the light reduction technology to cast the billet, the reduction amount is controlled at 2-5mm, the billet drawing speed is controlled at 1.0-1.4m / min, the casting overheat is controlled at 15-30°C, and the billet straightening temperature is controlled at 950±30°C.
Citation Information
Patent Citations
Normalized cryogenic steel at temperature of -50 DEG C and manufacturing method thereof
CN107557660A
Low-nickel steel for low-temperature storage tank and making method of low-nickel steel
CN110747409A
800MPa-grade hydrogen-induced crack resistant container steel plate and production method thereof
CN115369323A
590MPa-grade hydrogen induced cracking resistant electric resistance welding oil casing and manufacturing method thereof
CN116875880A
Ultralow-carbon-equivalent P690QL2 steel plate for hydrogen storage container and manufacturing method of ultralow-carbon-equivalent P690QL2 steel plate
CN117418158A