Method for intensively recovering valuable metals from waste PCBs (Printed Circuit Boards)
By adding oxidant to the NH3-(NH4)2SO4 system and reacting under ultrasonic shear conditions, the liquid-solid ratio and reaction conditions were optimized, and the problem of low zinc and nickel recycling efficiency in waste PCB boards was solved, and Cu and Zn were realized Efficient recycling of Ni and the enrichment of precious metals achieve green, clean and efficient production, reducing environmental pollution and energy consumption.
Patent Information
- Application Number
- CN202410986080.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has low efficiency in recycling zinc and nickel from waste PCB boards, and the traditional wet process poses potential risks to the environment, and is not very selective to precious metals, making it difficult to achieve efficient and green production.
By adding an oxidant to the NH3-(NH4)2SO4 system and reacting under ultrasonic shear conditions, the liquid-solid ratio, ammonia concentration and reaction temperature are optimized to form a complex of Cu, Zn and Ni, promote its leaching, and utilize ozone Improve the oxidative dissolution of metals, achieve efficient recycling of Cu, Zn and Ni, and at the same time enrich precious metals such as gold and silver in the leaching slag.
It improves the recovery rate of Cu, Zn and Ni, reduces process costs and energy consumption, avoids the production of nitrogen oxides, achieves green, clean and efficient metal recycling, and the leaching liquid can be recycled, reducing environmental pollution.
Smart Images

Figure BDA0004957432080000021
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a method for enhanced recovery of valuable metals from waste PCB boards, and belongs to the field of non-ferrous metal metallurgy. Background Art
[0002] With the vigorous development of production, the amount of discarded waste from electrical and electronic equipment is increasing, accounting for about 8% of urban waste, about 20-50 million tons per year. Therefore, electronic equipment waste needs to be properly treated. In recent years, environmental policies have paid more and more attention to the disposal of electronic waste. Circuit boards are an important part of waste electronic equipment waste. They are composed of components such as resistors, capacitors, transistors, diodes, microchips and integrated circuits. PCB boards contain base metals and precious metals, mainly copper, aluminum, tin, lead, zinc, silver and gold. From the perspective of economic value and environmental pollution protection, the recovery of valuable metals in waste PCB boards can promote the process of sustainable resource utilization.
[0003] The recovery of metals from waste PCBs is generally carried out through a combination of physical / mechanical, pyrometallurgical, hydrometallurgical, and biometallurgical processes. Hydrometallurgical processes are usually used to recover metals. This treatment method has the advantages of simplicity, low process cost, and small scale of operation. The hydrometallurgical process mainly selects specific leaching agents to extract soluble components from solids. Usually, they are reagents that can react with certain metals in waste PCBs. The most common ones are sulfuric acid, nitric acid, hydrochloric acid, or mixtures thereof. Common acids are not very selective for metals. Reagents or mixtures such as chlorides, thioureas, cyanides, glycine, and thiosulfates have strong selectivity for precious metals. Among them, the ammonia-ammonium sulfate system has good selectivity for copper, and the leaching residue can enrich precious metals such as gold and silver, which has great advantages. However, while ensuring a high leaching rate of copper, nickel and zinc must be recovered, and the consumption of ammonia is relatively large. Summary of the invention
[0004] In view of the problems and shortcomings of the above-mentioned prior art, the technical problem to be solved by the present invention is: a method for strengthening the recovery of valuable metals from waste PCB boards. The method provided by the present invention can effectively improve the process of zinc and nickel forming ammonium complexes with the leaching solution, and has a high recovery rate for Cu, Zn and Ni in PCB boards, and the leaching residue can be enriched with precious metals such as gold and silver, thereby achieving the purpose of green, clean and efficient production of PCB boards.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for enhanced recovery of valuable metals from waste PCBs comprises the following steps: stripping a microchip from the PCB and crushing it, reacting the metal-containing powder in NH3-(NH4)2SO4, adding different oxidants to a reaction tank through a gas cylinder, controlling the gas flow, liquid-solid ratio, ammonia concentration, ammonium sulfate concentration, reaction temperature and reaction time, and under ultrasonic shear strengthening, Cu, Zn and Ni of the microchip are coordinated with ammonia and enter into the solution, and Au and Ag are enriched in the slag phase.
[0007] According to the method, the particle size range of the microchips peeled from the PCB board after crushing is 80% below 1 mm and 20% above 1 mm.
[0008] In the described method, in the NH3-(NH4)2SO4 system solution, the concentration of NH3 (added by ammonia water) is 1-5 times the theoretical amount of Cu, Zn and Ni for complete coordination, the concentration of (NH4)2SO4 is 0.1-1 times the added concentration of NH3, the preferred NH3 concentration is 2-3 times the theoretical amount for complete coordination, and the preferred (NH4)2SO4 concentration is 0.5-1 times the added concentration of NH3.
[0009] In the method, the oxidant is hydrogen peroxide, bottled air, pure oxygen and ozone, and the air flow rate is 0.5-5L / min. Preferably, the oxidant is hydrogen peroxide and ozone, and the air flow rate is 0.5-2L / min.
[0010] In the method, during the reaction process, the liquid-to-solid ratio ranges from 10:1 to 80:1, the leaching reaction temperature is 30-80°C, and the reaction time is 0.5-3h. Preferably, the liquid-to-solid ratio ranges from 20:1 to 50:1, the leaching reaction temperature is 40-70°C, and the reaction time is 2-3h.
[0011] In the method, the ultrasonic frequency of the ultrasonic coupling is 20-400kHz, the ultrasonic power is 10-300W, and the shear rate is 2000-10000rpm. Preferably, the ultrasonic frequency is 50-200kHz, the ultrasonic power is 50-150W, and the shear rate is preferably 5000-8000rpm.
[0012] Principles and advantages
[0013] The method of the present invention realizes high-efficiency leaching of copper by optimizing the NH3-(NH4)2SO4 system. In conventional leaching of PCB, zinc and nickel are often not effectively recovered. Under this system, Cu, Zn and Ni elements can be leached with NH4 - Form coordination to generate Cu(NH3)4 2+ ,Zn(NH3)4 2+ and Ni(NH3)6 2+The complex enters the solution. Taking the oxidation coordination of copper as an example, see formula (1-2). Ozone is innovatively introduced. The introduction of oxidizing substances is conducive to the oxidation and dissolution of metal elements. The introduction of ultrasonic shearing enhancement method effectively increases the leaching rate of Cu, Zn and Ni. The principle is that ultrasonic waves can effectively separate metal particles and other impurities, thereby promoting the oxidation and dissolution reaction of metals. On the other hand, the introduction of shear will effectively promote the solid-liquid contact area while increasing the kinetics of the reaction between copper, zinc and nickel and ammonium ions, promoting the leaching and recovery of copper, zinc and nickel. In addition, precious metals such as gold and silver are greatly enriched in the leaching residue.
[0014] Cu+H2O2→CuO+H2O (1)
[0015] CuO+2NH3·H2O+ (NH4)2SO4→Cu(NH3)4 2+ +3H2O+SO4 2- (2)
[0016] In terms of recycling valuable metals from waste PCBs, the method of the present invention uses nitric acid as an oxidant and solution, compared with the traditional wet treatment process, to avoid the potential risk of nitrogen oxides generated during the leaching and heating process to the environment; sulfuric acid, hydrochloric acid or nitric acid has poor selectivity for metals when used as a leaching agent, providing a method for efficiently recycling valuable metals Cu, Zn and Ni from PCB microchips, with a simpler process and a lower energy consumption method, and the leachate can be recycled without generating waste gas and waste water. The present invention is of great significance to promoting the production technology progress, energy saving and consumption reduction, and environmental protection of waste PCB recycling in my country. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] none Specific implementation plan
[0018] The following examples are intended to further illustrate the present invention but are not intended to limit the present invention.
[0019] Example 1
[0020] The raw material is waste PCB provided by a company. The main metal components and contents of the microchips peeled from it are as follows:
[0021]
[0022] The microchip was peeled off from the waste PCB board, ground, crushed and sieved to obtain two types of particle sizes, >1mm and <1mm, of which more than 80% of the particle size was <1mm. 200g of microchip powder with a particle size <1mm was weighed this time, the NH3 concentration was 2 times the theoretical amount of complete coordination, and the (NH4)2SO4 concentration was 1 times the NH3 addition concentration. The liquid-solid ratio was 20:1, and ozone was transported to the bottom of the leachate through a hose for reaction. The ozone flow was controlled at 0.5L / min, the ultrasonic frequency was 100kHz, the ultrasonic power was 100W, the shear rate was 8000rpm, and the reaction temperature and time were 50℃ and 2h, respectively. After the reaction, the leachate and leach residue were obtained. The leachate was analyzed to determine the content of Cu, Zn and Ni. The calculated leaching rates of Cu, Zn and Ni reached 97%, 92% and 86%, respectively. The leach residue was dried and weighed for analysis, and the content of Au and Ag elements was 0.05% and 0.02%, respectively.
[0023] Example 2
[0024] Use the waste PCB as shown in Example 1 as raw material, weigh 200g of microchip powder with a particle size of <1mm, the NH3 concentration is 2.5 times the theoretical amount of complete coordination, and the (NH4)2SO4 concentration is 1 times the NH3 addition concentration. The liquid-solid ratio is 30:1, and ozone is transported to the bottom of the leachate through a hose for reaction. The ozone flow rate is controlled at 2L / min, the ultrasonic frequency is 150kHz, the ultrasonic power is 150W, the shear rate is 5000rpm, and the reaction temperature and time are 60°C and 2.5h respectively. After the reaction, the leachate and leach residue are obtained. The leachate is analyzed to determine the content of Cu, Zn and Ni. The calculated leaching rates of Cu, Zn and Ni are 98.7%, 93.8% and 86% respectively. The leach residue is dried and weighed for analysis, and the content of Au and Ag elements is 0.05% and 0.04%.
[0025] Example 3
[0026] Use the waste PCB as shown in Example 1 as raw material, weigh 200g of microchip powder with a particle size of <1mm, the NH3 concentration is 3 times the theoretical amount of complete coordination, and the (NH4)2SO4 concentration is 1 times the NH3 addition concentration. The liquid-solid ratio is 50:1, and ozone is transported to the bottom of the leachate through a hose for reaction. The ozone flow rate is controlled at 1L / min, the ultrasonic frequency is 200kHz, the ultrasonic power is 125W, the shear rate is 6500rpm, and the reaction temperature and time are 40°C and 3h respectively. After the reaction, the leachate and leach residue are obtained. The leachate is analyzed to determine the content of Cu, Zn and Ni. The calculated leaching rates of Cu, Zn and Ni are 98%, 94% and 88% respectively. The leach residue is dried and weighed for analysis, and the content of Au and Ag elements is 0.06% and 0.03%.
[0027] Comparative Example 1 (Particle Size Range Selection)
[0028] Waste PCB as shown in Example 1 was used as raw material. 200g of microchip powder with a particle size of >1mm was weighed this time, the NH3 concentration was 2 times the theoretical amount of complete coordination, and the (NH4)2SO4 concentration was 1 times the NH3 addition concentration. The liquid-solid ratio was 20:1, and ozone was transported to the bottom of the leachate through a hose for reaction. The ozone flow was controlled at 0.5L / min, the ultrasonic frequency was 100kHz, the ultrasonic power was 100W, the shear rate was 8000rpm, and the reaction temperature and time were 50°C and 2h, respectively. After the reaction, the leachate and leach residue were obtained. The leachate was analyzed to determine the content of Cu, Zn and Ni. The calculated leaching rates of Cu, Zn and Ni reached 94%, 89% and 84%, respectively. The leach residue was dried and weighed for analysis, and the content of Au and Ag elements was 0.03% and 0.01%.
[0029] Comparative Example 2 (no ultrasonic enhancement)
[0030] Waste PCB as shown in Example 1 was used as raw material. 200g of microchip powder with a particle size of <1mm was weighed this time, the NH3 concentration was twice the theoretical amount of complete coordination, and the (NH4)2SO4 concentration was 1 times the NH3 addition concentration. The liquid-solid ratio was 20:1, and ozone was transported to the bottom of the leachate through a hose for reaction. The ozone flow was controlled at 0.5L / min, the shear rate was 8000rpm, and the reaction temperature and time were 50°C and 2h, respectively. After the reaction, leachate and leach residue were obtained. The leachate was analyzed to determine the content of Cu, Zn and Ni. The calculated leaching rates of Cu, Zn and Ni reached 92%, 88% and 84%, respectively. The leach residue was dried and weighed for analysis, and the content of Au and Ag elements was 0.05% and 0.03%.
[0031] Comparative Example 3 (without shear strengthening)
[0032] Waste PCB as shown in Example 1 was used as raw material. 200g of microchip powder with a particle size of <1mm was weighed this time, the NH3 concentration was 2 times the theoretical amount of complete coordination, and the (NH4)2SO4 concentration was 1 times the NH3 addition concentration. The liquid-solid ratio was 20:1, and ozone was transported to the bottom of the leachate through a hose for reaction. The ozone flow was controlled at 0.5L / min, the ultrasonic frequency was 100kHz, the ultrasonic power was 100W, and the reaction temperature and time were 50°C and 2h, respectively. After the reaction, the leachate and leach residue were obtained. The leachate was analyzed to determine the content of Cu, Zn and Ni. The calculated leaching rates of Cu, Zn and Ni reached 94%, 89% and 86%, respectively. The leach residue was dried and weighed for analysis, and the content of Au and Ag elements was 0.06% and 0.035%.
[0033] Comparative Example 4 (without ultrasonic coupling shear strengthening)
[0034] Waste PCB as shown in Example 1 was used as raw material. 200g of microchip powder with a particle size of <1mm was weighed this time, the NH3 concentration was twice the theoretical amount of complete coordination, and the (NH4)2SO4 concentration was 1 times the NH3 addition concentration. The liquid-solid ratio was 20:1, and ozone was transported to the bottom of the leachate through a hose for reaction. The ozone flow rate was controlled at 0.5L / min, and the reaction temperature and time were 50°C and 2h, respectively. After the reaction, leachate and leach residue were obtained. The leachate was analyzed to determine the content of Cu, Zn and Ni. The calculated leaching rates of Cu, Zn and Ni reached 89%, 86% and 78%, respectively. The leach residue was dried and weighed for analysis, and the content of Au and Ag elements was 0.045% and 0.024%.
Claims
1. A method for intensively recovering valuable metals from waste PCBs, characterized in that: The peeled microchips are crushed and ground to obtain metal powders, which are then separated by size through corresponding sieves. The metal powders are leached by introducing oxidizing gas into the NH3-(NH4)2SO4 system solution under external field coupling enhancement conditions. As the reaction proceeds, copper, zinc and nickel elements enter the solution.
2. The method according to claim 1, characterized in that: The metal-containing powder obtained by crushing and grinding the microchips on the PCB board is separated by size through a vibrating shaker and corresponding sieves. The particle size range is divided into two particle size ranges: <1mm and >1mm.
3. The method according to claim 1, characterized in that: The concentration of the added NH3 (added by ammonia water) is 1-5 times the theoretical amount of Cu, Zn and Ni for complete coordination, the concentration of (NH4)2SO4 is 0.1-1 times the concentration of NH3 addition, and the liquid-to-solid ratio of the raw material and the NH3-(NH4)2SO4 solution ranges from 10:1 to 80:
1.
4. The method according to claim 1, characterized in that: The oxidizing gas includes one of hydrogen peroxide, bottled air, pure oxygen and ozone, and the gas flow rate is 0.5-5L / min.
5. The method according to claim 1, characterized in that: The external field coupling enhancement condition is ultrasonic coupling shear enhancement.
6. The method according to claim 1 and claim 5, characterized in that: The ultrasonic coupling has an ultrasonic frequency of 20-400 kHz, an ultrasonic frequency of 10-300 W, and a shear rate of 2000-10000 rpm.
7. The method according to claim 1, characterized in that: The leaching reaction temperature is 30-80°C, and the reaction time is 0.5-3h.