Iron-copper diatomic catalyst and preparation method thereof
The iron-copper diatomic catalyst supported on porous carbon was prepared by self-assembly and pickling-carbonizing the metal iron salt and copper salt with sulfur source in an electrocatalyst, and the single-atomic catalyst was solved in ORR The problem of activity restriction and inactivation achieves efficient electrocatalytic oxygen reduction and is suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202410978713.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Single-atom catalysts have activity limitations and inactivation problems in catalytic redox reactions (ORRs), making it difficult to effectively drive the multi-electron and multi-proton transfer processes, and it is difficult to prepare diatomic catalysts with clear structure and excellent performance through simple and controllable methods.
By self-assembling metal iron salt and metal copper salt with sulfur source in oil bath heating, combining pickling and carbonization processes, an iron-copper diatom catalyst loaded on porous carbon is prepared, using the synergistic action of adjacent metal sites. Regulate active sites and improve electrocatalytic redox efficiency.
The prepared iron-copper diatom catalyst has a high specific surface area and more active sites, which significantly improves the electrocatalytic oxygen reduction efficiency, and is simple in process and strong repeatability, making it suitable for large-scale industrial production.
Smart Images

Figure CN118932392A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochemical reduction catalysts, and more specifically, to an iron-copper diatomic catalyst and a preparation method thereof. Background Art
[0002] In recent years, electrocatalytic technology has been widely used in the fields of energy conversion and storage, environmental governance, etc. Especially in the processes of hydrogen production, fuel cells, carbon dioxide reduction, etc., the performance of electrocatalysts directly affects the efficiency and stability of the entire system. Among them, single-atom catalysts have become a research hotspot in photocatalysis, thermal catalysis and electrocatalysis due to their good catalytic performance due to their 100% atomic utilization, highly unsaturated coordination and unique atomic structure. However, it is difficult for single-atom catalysts to break the severe limitation of the linear adsorption relationship of oxygen-containing intermediates on catalytic activity in the catalytic oxygen reduction reaction (ORR), inhibiting the kinetic rate of the catalytic reaction. In addition, the density of single-atom active sites is low, and they are easily occupied by intermediates, causing serious deactivation of the catalyst, making it difficult for a single active center to effectively drive multi-electron and multi-proton transfer processes.
[0003] Studies have shown that diatomic catalysts have higher activity than homologous single-atom catalysts. Diatomic catalysts contain two active centers that can be the same or different, either transition metals and transition metals, or transition metals and rare earth metals, which greatly expands the types and structures of active sites, and can regulate active sites for specific catalytic reactions. Compared with single-atom catalysts, Fe-Ni, Fe-Co and Fe-Zn dimetallic sites can improve ORR activity through synergistic effects. The electrochemical performance of the catalyst can be effectively improved by adjusting the atomic size of the catalyst. On the one hand, it can improve the atomic utilization and exposure of active sites, and increase the number of metal active sites; on the other hand, diatomic atoms have adjacent metal active sites and the mutual synergistic effect between adjacent metals reduces the activation energy barrier of the transition state, thereby improving the electrocatalytic efficiency.
[0004] Therefore, how to prepare diatomic catalysts with clear structures and excellent performance through simple and controllable methods remains a major challenge in current research. Summary of the invention
[0005] In view of the above, the present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides an iron-copper diatomic catalyst and a preparation method thereof. The iron-copper diatomic catalyst prepared by the preparation method of the present invention has a high specific surface area and a larger number of active sites, and can effectively improve the electrocatalytic oxygen reduction efficiency. At the same time, the preparation method has a simple process flow and is suitable for application in large-scale industrial production.
[0006] To this end, in a first aspect, an embodiment of the present invention provides an iron-copper diatomic catalyst, wherein the iron-copper diatomic catalyst is formed by self-assembly of a metal iron salt and a metal copper salt with a sulfur source by oil bath heating, and then through a pickling and carbonization process.
[0007] In a second aspect, an embodiment of the present invention provides a method for preparing the iron-copper diatomic catalyst provided in the first aspect, the method comprising: step S1: weighing a certain amount of sulfur source and transferring it to a flask containing 30-50 mL of water, then placing it in an oil bath and heating and stirring, taking a certain amount of magnesium chloride hexahydrate, potassium hydroxide, metal iron salt, and metal copper salt in aqueous solution or ethanol solution and adding them to the flask at a certain time and in order, mixing and reacting for a certain time, adding a certain amount of sugar, stirring for a second time and cooling naturally, and freeze-drying the obtained suspension to obtain a dry material; step S2: placing the dry material in a tubular furnace under a nitrogen atmosphere, heating it once and keeping it warm for a certain time, and then heating it twice and keeping it warm for a certain time to obtain a primary carbide; step S3: pickling the primary carbide with a nitric acid solution for a certain time, then washing it with deionized water to neutrality, and then filtering it with ethanol, drying it to obtain an intermediate, placing the intermediate in a tubular furnace under a nitrogen atmosphere for secondary carbonization to obtain the iron-copper diatomic catalyst.
[0008] Preferably, in step S1, the heating temperature is 55-95° C. and the stirring time is 20 min.
[0009] Preferably, in step S1, the reaction time is 0.5-5 h, the secondary stirring time is 2-8 h, and the freeze-drying time is 20 h.
[0010] Preferably, in step S1, the sulfur source is thiosemicarbazide; the metal iron salt is ferric acetylacetonate; the metal copper salt is copper acetate monohydrate; and the sugar is one or more of chitosan, agarose, glucose, and the like.
[0011] Preferably, in step S1, the mass ratio of the thiosemicarbazide, the magnesium chloride hexahydrate, the potassium hydroxide, the ferric acetylacetonate, the cupric acetate monohydrate and the chitosan added is (1-3): (1-3): (0.5-1.5): (0.1-0.36): (0-0.2): (0.2-0.6).
[0012] Preferably, in step S1, the drying material comprises self-assembled thiosemicarbazide-chitosan-iron-copper precursor mixed hydrogel, magnesium hydroxide and potassium chloride.
[0013] Preferably, in step S2, the heating rate is 2-5°C / min, the heating temperature is 350-450°C, and the heating holding time is 1-3h.
[0014] Preferably, in step S2, the secondary heating heating rate is 4-10°C / min, the secondary heating temperature is 800-1000°C, and the secondary heating insulation time is 1-3h.
[0015] Preferably, in step S3, the concentration of the nitric acid solution is 0.1-3 mol / L, the pickling time is 10-15 h, the heating rate during the secondary carbonization is 2-5°C / min, the heating temperature is 800-1200°C, and the insulation time is 1-3 h.
[0016] The iron-copper diatomic catalyst and preparation method thereof provided in the embodiment of the present invention synthesizes an iron-copper diatomic catalyst supported on porous carbon through an aggregation-redispersion approach, and utilizes the mutual synergistic effect of adjacent metal sites during the preparation process to achieve effective regulation of diatomic active sites to reduce the transition state energy barrier, thereby improving the electrocatalytic oxygen reduction efficiency. In addition, by adjusting the geometric structure and coordination environment of the iron-copper double site, the prepared iron-copper diatomic catalyst has a high specific surface area and more active sites, which can effectively improve the electrocatalytic oxygen reduction efficiency. At the same time, the preparation method is simple in process, highly repeatable, and stable, and is suitable for application in large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 A flow chart of a method for preparing an iron-copper diatomic catalyst provided in an embodiment of the present invention.
[0018] Figure 2 The X-ray diffraction (XRD) pattern of the iron-copper diatomic catalyst prepared in Example 1 of the present invention;
[0019] Figure 3 A transmission electron microscope (TEM) image of the iron-copper diatomic catalyst provided in Example 1 of the present invention;
[0020] Figure 4 This is an X-ray energy spectrum (EDS) image of the iron-copper diatomic catalyst provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0021] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0022] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or letters in different examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can appreciate the applicability of other processes and / or the use of other materials.
[0023] The object of the present invention is to provide an iron-copper diatomic catalyst and a preparation method thereof, and an iron-copper diatomic catalyst supported on porous carbon is synthesized by an aggregation-redispersion approach. Specifically, the first embodiment of the present invention provides an iron-copper diatomic catalyst, wherein the iron-copper diatomic catalyst is self-assembled by oil bath heating with a metal iron salt and a metal copper salt and a sulfur source, and then through a pickling and carbonization process, an iron-copper diatomic catalyst is finally formed. The iron-copper diatomic catalyst has a high specific surface area and a larger number of active sites, and can effectively improve the efficiency of electrocatalytic oxygen reduction.
[0024] The second embodiment of the present invention provides a method for preparing an iron-copper diatomic catalyst, such as Figure 1 As shown, the preparation method comprises the following steps:
[0025] Step S1: Weigh a certain amount of sulfur source and transfer it to a flask filled with 30-50 mL of water, then put it into an oil bath pot for heating and stirring, take a certain amount of magnesium chloride hexahydrate, potassium hydroxide, metal iron salt, metal copper salt aqueous solution or ethanol solution and add it to the flask at a certain time and in a certain order, after mixing and reacting for a certain time, add a certain amount of sugar, stir twice and cool naturally, and then freeze-dry the obtained suspension to obtain a dry material;
[0026] The heating temperature can be 55-95°C, the stirring time can be 20 minutes, the reaction time can be 0.5-5 hours, the secondary stirring time can be 2-8 hours, and the freeze drying time can be 20 hours. In addition, the early and middle oil bath steps in the oil bath pot are condensation reflux, and the late oil bath steps are open (except ethanol).
[0027] In this embodiment, the sulfur source can be thiosemicarbazide; the metal iron salt can be iron acetylacetonate; the metal copper salt can be copper acetate monohydrate; the sugar can be one or more of chitosan, agarose, glucose, etc.; the drying material includes self-assembled thiosemicarbazide-chitosan-iron-copper precursor mixed hydrogel, magnesium hydroxide and potassium chloride. The mass ratio of the thiosemicarbazide, the magnesium chloride hexahydrate, the potassium hydroxide, the iron acetylacetonate, the copper acetate monohydrate, and the chitosan is (1-3): (1-3): (0.5-1.5): (0.1-0.36): (0-0.2): (0.2-0.6). Specifically, the amount of thiosemicarbazide added is 1-3g; the amounts of magnesium chloride hexahydrate and potassium hydroxide added are 1-3g and 0.5-1.5g respectively; the amount of ferric acetylacetonate added is 0.1-0.36g; the amount of cupric acetate monohydrate added is 0-0.2g; and the amount of chitosan added is 0.2-0.6g.
[0028] Step S2: placing the dried material in a tubular furnace under a nitrogen atmosphere, heating it once and then keeping it warm for a certain period of time, and then heating it twice and then keeping it warm for a certain period of time to obtain a primary carbide;
[0029] Among them, the primary heating heating rate can be 2-5℃ / min, the primary heating temperature can be 350-450℃, and the primary heating insulation time can be 1-3h; the secondary heating heating rate can be 4-10℃ / min, the secondary heating temperature can be 800-1000℃, and the secondary heating insulation time can be 1-3h.
[0030] In step S2, the gel in the dried material can be pyrolyzed once to decompose magnesium hydroxide, reconstruct potassium chloride, and carbonize the iron-copper precursor, thereby using magnesium oxide and potassium chloride as templates to prepare a porous carbide containing an iron-copper metal mixture.
[0031] Step S3: The primary carbide is pickled with a nitric acid solution for a certain period of time, then washed with deionized water until neutral, filtered with ethanol, and dried to obtain an intermediate, and the intermediate is placed in a tubular furnace under a nitrogen atmosphere for secondary carbonization to obtain the iron-copper diatomic catalyst.
[0032] The concentration of the nitric acid solution may be 0.1-3 mol / L, the pickling time may be 10-15 h, the heating rate during secondary carbonization may be 2-5° C. / min, the heating temperature may be 800-1200° C., and the insulation time may be 1-3 h.
[0033] In step S3, the template and excess metal particles or metal oxides can be removed by acid washing.
[0034] The preparation method of the iron-copper diatomic catalyst provided in the embodiment of the present invention synthesizes an iron-copper diatomic catalyst supported on porous carbon by an aggregation-redispersion approach, and utilizes the mutual synergistic effect of adjacent metal sites during the preparation process to achieve effective regulation of diatomic active sites to reduce the transition state energy barrier, thereby improving the electrocatalytic oxygen reduction efficiency. In addition, by adjusting the geometric structure and coordination environment of the iron-copper double site, the purpose of optimizing the catalytic activity of the catalyst is achieved. At the same time, the preparation method is simple in process, highly repeatable, and stable, and is suitable for application in large-scale industrial production.
[0035] The specific process and effect of the preparation method of the iron-copper diatomic catalyst of the present invention are further described in detail below in conjunction with some specific embodiments, but are not limited to the protection scope of the present invention.
[0036] Example 1
[0037] This embodiment provides a method for preparing an iron-copper diatomic catalyst. The iron-copper diatomic catalyst prepared in this embodiment is a Fe-Cu-NC (KJT-Fe-Cu-NC) catalyst, which comprises the following steps:
[0038] Pour 40 mL of water into a three-necked flask, then put it into an oil bath, add 3 g of thiosemicarbazide into the three-necked flask (condensation reflux), heat to 80 ° C and stir for 20 min, then add 2.0 g of magnesium chloride hexahydrate (dissolved in 10 mL of aqueous solution) and 1.5 g of potassium hydroxide (dissolved in 7.5 mL of aqueous solution); after reacting for 15 min, add 0.30 g of ferric acetylacetonate (dissolved in 40 mL of ethanol solution) into the three-necked flask; after vigorous stirring for 30 min, dissolve 0.6 g of chitosan into the solution, then The mixture was stirred continuously at 80°C for 2h (open) and then cooled naturally; the obtained suspension was aged for 10h and then freeze-dried to obtain a dry material; the dry material was placed in a tubular furnace under a nitrogen atmosphere and carbonized at 350°C for 1h and 950°C for 2h respectively; the product was then leached in a 3mol / L nitric acid solution at 80°C for 12h to obtain an intermediate; and then secondary pyrolysis was performed at 950°C to finally obtain the Fe-Cu-NC (KJT-Fe-Cu-NC) catalyst.
[0039] Figure 2 The X-ray diffraction (XRD) pattern of the iron-copper diatomic catalyst prepared in Example 1 of the present invention;
[0040] Figure 3 A transmission electron microscope (TEM) image of the iron-copper diatomic catalyst provided in Example 1 of the present invention;
[0041] Figure 4This is an X-ray energy spectrum (EDS) image of the iron-copper diatomic catalyst provided in Example 1 of the present invention.
[0042] Example 2
[0043] This embodiment provides a method for preparing an iron-copper diatomic catalyst. The iron-copper diatomic catalyst prepared in this embodiment is a Fe-Cu-NC (QZ-Fe-Cu-NC) catalyst, which comprises the following steps:
[0044] Pour 40 mL of water into a three-necked flask, then put it into an oil bath, add 3 g of thiosemicarbazide into the three-necked flask (condensation reflux), heat to 80°C and stir for 20 min; add 2.0 g of magnesium chloride hexahydrate (dissolved in 10 mL of aqueous solution) and 1.5 g of potassium hydroxide (dissolved in 7.5 mL of aqueous solution); after reacting for 15 min, add 0.30 g of ferric acetylacetonate (dissolved in 40 mL of ethanol solution) into the three-necked flask; after vigorous stirring for 30 min, dissolve 0.54 g of chitosan into the solution, Then, the mixture was stirred continuously at 80°C for 2h (open) and then cooled naturally; the obtained suspension was aged for 10h and then freeze-dried to obtain a dry material; the dry material was placed in a tubular furnace under a nitrogen atmosphere and carbonized at 350°C for 1h and 950°C for 2h respectively; the product was then leached in a 3mol / L nitric acid solution at 80°C for 12h to obtain an intermediate; and then, after secondary pyrolysis at 950°C, the Fe-Cu-NC (QZ-Fe-Cu-NC) catalyst was finally obtained.
[0045] In summary, the iron-copper diatomic catalyst and preparation method thereof provided in the embodiment of the present invention synthesizes an iron-copper diatomic catalyst supported on porous carbon through an aggregation-redispersion approach, and utilizes the mutual synergistic effect of adjacent metal sites during the preparation process to achieve effective regulation of diatomic active sites to reduce the transition state energy barrier, thereby improving the electrocatalytic oxygen reduction efficiency. In addition, by adjusting the geometric structure and coordination environment of the iron-copper double site, the prepared iron-copper diatomic catalyst has a high specific surface area and more active sites, which can effectively improve the electrocatalytic oxygen reduction efficiency. At the same time, the preparation method is simple in process, highly repeatable, and stable, and is suitable for application in large-scale industrial production.
[0046] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0047] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. An iron-copper diatomic catalyst, It is characterized in that The iron-copper diatomic catalyst is formed by self-assembly of metal iron salt, metal copper salt and sulfur source by oil bath heating, and then by acid washing and carbonization process.
2. A method for preparing the iron-copper diatomic catalyst as claimed in claim 1, It is characterized in that The preparation method comprises: Step S1: Weigh a certain amount of sulfur source and transfer it to a flask filled with 30-50 mL of water, then put it into an oil bath pot for heating and stirring, take a certain amount of magnesium chloride hexahydrate, potassium hydroxide, metal iron salt, metal copper salt aqueous solution or ethanol solution and add it to the flask at a certain time and in a certain order, after mixing and reacting for a certain time, add a certain amount of sugar, stir twice and cool naturally, and then freeze-dry the obtained suspension to obtain a dry material; Step S2: placing the dried material in a tubular furnace under a nitrogen atmosphere, heating it once and then keeping it warm for a certain period of time, and then heating it twice and then keeping it warm for a certain period of time to obtain a primary carbide; Step S3: The primary carbide is pickled with a nitric acid solution for a certain period of time, then washed with deionized water until neutral, filtered with ethanol, and dried to obtain an intermediate, and the intermediate is placed in a tubular furnace under a nitrogen atmosphere for secondary carbonization to obtain the iron-copper diatomic catalyst.
3. The method for preparing the iron-copper diatomic catalyst according to claim 2, It is characterized in that In the step S1, the heating temperature is 55-95° C. and the stirring time is 20 min.
4. The method for preparing the iron-copper diatomic catalyst according to claim 2, It is characterized in that In the step S1, the reaction time is 0.5-5 h, the secondary stirring time is 2-8 h, and the freeze-drying time is 20 h.
5. The method for preparing the iron-copper diatomic catalyst according to claim 2, It is characterized in that In step S1, the sulfur source is thiosemicarbazide; the metal iron salt is ferric acetylacetonate; the metal copper salt is copper acetate monohydrate; and the sugar is one or more of chitosan, agarose, glucose, and the like.
6. The method for preparing the iron-copper diatomic catalyst according to claim 5, It is characterized in that The mass ratio of the thiosemicarbazide, the magnesium chloride hexahydrate, the potassium hydroxide, the ferric acetylacetonate, the cupric acetate monohydrate, and the chitosan added is (1-3): (1-3): (0.5-1.5): (0.1-0.36): (0-0.2): (0.2-0.6).
7. The method for preparing the iron-copper diatomic catalyst according to claim 2, It is characterized in that In the step S1, the drying material includes self-assembled thiosemicarbazide-chitosan-iron-copper precursor mixed hydrogel, magnesium hydroxide and potassium chloride.
8. The method for preparing the iron-copper diatomic catalyst according to claim 2, It is characterized in that In the step S2, the heating rate is 2-5°C / min, the heating temperature is 350-450°C, and the heating insulation time is 1-3h.
9. The method for preparing the iron-copper diatomic catalyst according to claim 2, It is characterized in that In the step S2, the secondary heating heating rate is 4-10°C / min, the secondary heating temperature is 800-1000°C, and the secondary heating insulation time is 1-3h.
10. The method for preparing the iron-copper diatomic catalyst according to claim 2, It is characterized in that In the step S3, the concentration of the nitric acid solution is 0.1-3 mol / L, the pickling time is 10-15 h, the heating rate during the secondary carbonization is 2-5°C / min, the heating temperature is 800-1200°C, and the insulation time is 1-3 h.
Citation Information
Cited By
Oxygen reduction and carbon dioxide reduction electrocatalyst and preparation method and application thereof
CN121653744A