Sr-doped molybdenum diselenide mesoporous nanosheet structure material as well as preparation method and application thereof

Synthesis of Sr-doped molybdenum diselenide mesoporous nanosheet structural materials on a one-step liquid phase method on a foamed copper substrate, the problems of existing catalysts being low in CO2ER were solved, and high-efficiency and low-cost methanol were achieved Production, suitable for flow cell and membrane battery applications.

CN118932393APending Publication Date: 2024-11-12ANHUI NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982817.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult for existing catalysts to achieve high selectivity and high current density methanol production in carbon dioxide electrocatalytic reduction reaction (CO2ER), and there are problems with the use and preparation of precious metals, resulting in low energy efficiency and high cost.

Method used

Synthesize Sr-doped molybdenum diselenide mesoporous nanosheet structure materials on foamed copper substrate by one-step liquid phase method. By adjusting the electronic structure and active sites, the selectivity and current density of the catalyst are improved, and in the flow cell and membrane cell Applied in.

Benefits of technology

It realizes methanol production with low potential, high selectivity and high energy efficiency at high current density, and is simple in preparation process and low in cost, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932393A_ABST
    Figure CN118932393A_ABST
Patent Text Reader

Abstract

The invention provides a Sr-doped molybdenum diselenide mesoporous nanosheet structure material as well as a preparation method and application thereof. The Sr-doped molybdenum diselenide mesoporous nanosheet structure material is prepared by putting a molybdenum source into water and ethanol, putting a selenium source into a reducing agent solution, mixing the two solutions, adding a strontium source, putting foamy copper and performing solvothermal reaction. Compared with the prior art, the thin mesoporous nanosheet structure is beneficial to exposure of side active sites; sr < 2 + > is doped, an electronic structure is adjusted, exposure of active sites is increased, multiple active sites are formed, charge separation efficiency is improved, intermediate species and adsorption behaviors thereof are optimized, and catalytic kinetics is accelerated. Sr is doped on molybdenum diselenide crystal lattices to generate rich selenium vacancies, adsorption and activation of CO2 molecules are promoted, and the CO2 molecules are converted into a series of related C1 intermediates to generate methanol. In a flow cell and a membrane battery, CO2 can be electrically reduced into a methanol liquid product with high selectivity and high current density, and excellent activity, selectivity and stability and high energy efficiency in the membrane battery are shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nano material preparation methods and electrocatalytic applications, and specifically relates to an Sr-doped molybdenum diselenide mesoporous nanosheet structure material and a preparation method and application thereof. Background Art

[0002] The electrocatalytic reduction reaction of carbon dioxide (CO 2 ER) can synthesize high energy density fuels and basic chemicals. Methanol, as a CO 2 ER Liquid C 1 The product is a green fuel and chemical raw material with high energy density. 2 Great progress has been made in the ER to methanol process, but competition from other products with similar intermediates in multiple steps and the active components in the catalyst are not sufficient in CO 2 It is difficult to be stable under ER conditions, so it is still a considerable challenge to simultaneously achieve high selectivity and methanol production at high current density.

[0003] At present, some catalysts such as FeP, BP, Pd / SnO 2 、Cu / Cu 2 O, metal organic frameworks, and cobalt phthalocyanine modified single-walled carbon nanotubes (CoPc / SWCNTs), etc., have achieved more than 50% methanol selectivity in H-type electrolyzers by regulating the active sites of the catalysts to control the evolution of reaction intermediates, but the corresponding methanol partial current density is relatively small. The use of ionic liquid electrolytes can improve CO 2 solubility and adsorption to achieve CO 2 ER has high selectivity and activity to methanol, but the expensive ionic liquids and additional costs of subsequent product separation hinder its industrial application.

[0004] To this end, researchers use flow cells with gas diffusion electrodes to improve the conversion efficiency of carbon dioxide at high current density by promoting the mass transfer of carbon dioxide. However, only a few catalysts are currently used in flow cells to produce methanol. For example, CuGa 2 Intermetallic compounds, CoPc / SWCNTs, Pd / MnO 2 , Mn doping VS 2 Moreover, the catalysts that can produce methanol with high selectivity at high current density are limited to Pd / MnO 2 The use of expensive precious metals and the cumbersome step-by-step preparation process limit the further application of this catalyst. At the same time, the large distance between the cathode and anode in the flow cell device leads to increased resistance, which in turn leads to significant energy loss. The membrane cell electrolyzer (MEA) with a "zero gap" structural feature can reduce the distance between the electrodes, reduce the resistance of the device, and the use of no cathode liquid avoids CO2 The mass transfer limitation of CO 2 Energy efficiency of ER.

[0005] Currently, the catalysts that can be used in membrane batteries to produce methanol are limited to Cu 2 NCN and Pd / MnO 2 Several catalysts such as Cu 2 NCN catalyst has a variety of liquid products, resulting in low methanol current density and high downstream separation cost; Pd / MnO 2 Catalysts have the problem of using expensive precious metals and complicated preparation processes. Therefore, it is necessary to explore catalysts that can convert CO into CO with high selectivity and high current density in flow cells and membrane battery electrolyzers. 2 A low-cost catalyst for reduction to methanol for potential practical applications. Summary of the invention

[0006] The purpose of the present invention is to provide an Sr-doped molybdenum diselenide mesoporous nanosheet structure material and a preparation method thereof. The Sr-doped molybdenum diselenide mesoporous nanosheet structure material is synthesized on a foam copper substrate by a one-step liquid phase method. The preparation method is simple and efficient, suitable for industrial promotion, and has broad application prospects.

[0007] Another object of the present invention is to provide an application of Sr-doped molybdenum diselenide mesoporous nanosheet structure material, wherein the prepared Sr-doped molybdenum diselenide mesoporous nanosheet structure material is used as a CO 2 Applications of ER electrocatalysts, especially for CO 2 Application of ER electrocatalyst to produce methanol. It has the characteristics of low potential, high selectivity, good stability and high energy efficiency at high current density.

[0008] The specific technical solutions of the present invention are as follows:

[0009] A method for preparing a Sr-doped molybdenum diselenide mesoporous nanosheet structure material, the preparation method comprising:

[0010] A molybdenum source is placed in a mixed solvent of water and ethanol, and a selenium source is placed in a reducing agent solution. After the two solutions are mixed, a strontium source is added, and foam copper is placed in the solution to carry out a solvothermal reaction to obtain an Sr-doped molybdenum diselenide mesoporous nanosheet structure material.

[0011] The foam copper needs to be cleaned before use. The specific cleaning method is: first soak it in 6M hydrochloric acid for 15 minutes to remove the oxide film on the surface, and then clean it with deionized water and anhydrous ethanol; the cleaned foam copper is cut into a size of 2×3 cm when used.

[0012] The molar ratio of the strontium source, the molybdenum source and the selenium source is 0.04-0.12:1:2, preferably 0.08:1:2;

[0013] The molybdenum source and water are used in a ratio of 0.1 mol / L;

[0014] The strontium source is a soluble strontium salt, preferably Sr(NO 3 ) 2 ;

[0015] The molybdenum source is a soluble molybdenum salt, preferably Na 2 MoO 4 ·2H 2 O;

[0016] The selenium source is selenium powder;

[0017] The reducing agent solution is a hydrazine hydrate aqueous solution with a mass fraction of 50wt.%;

[0018] The volume ratio of the ethanol, water and reducing agent solution is 7.5-22.5:5-15:8-24, preferably 15:10:16;

[0019] The solvent thermal reaction conditions are 230-250°C for 23-25h, preferably 240°C for 24h;

[0020] The solvent thermal reaction is carried out in a reaction kettle lined with polytetrafluoroethylene;

[0021] During the solvothermal reaction, the copper foam was placed at an angle so that the sample could grow evenly on both sides of the copper foam.

[0022] Furthermore, after the solvothermal reaction, the product was naturally cooled to room temperature, washed and dried to obtain Sr-doped MoSe 2 Mesoporous nanosheet structure material; the washing step is: first washing with deionized water for 3 to 5 times, and then washing with anhydrous ethanol for 3 to 5 times; the drying step is: drying in a vacuum drying oven at 55 to 70°C for 4 to 8 hours.

[0023] The invention provides a Sr-doped molybdenum diselenide mesoporous nanosheet structure material, which is prepared by the above method. The morphology of the Sr-doped molybdenum diselenide mesoporous nanosheet structure material is a mesoporous nanosheet structure material in which mesopores with a size of 5 to 36 nm are distributed on nanosheets with a lateral size of 500 to 600 nm and a thickness of 6 to 10 nm; the Sr doping accounts for 2.9% to 8.7% of the total atomic weight of Sr and Mo.

[0024] The invention provides an application of a Sr-doped molybdenum diselenide mesoporous nanosheet structure material as an electrocatalytic carbon dioxide reduction reaction (CO 2 ER) electrocatalysts, especially for CO 2 Application of ER electrocatalyst to produce methanol.

[0025] The specific application method is as follows: the Sr-doped molybdenum diselenide mesoporous nanosheet structure material ultrasonically removed from the foam copper is dispersed in isopropanol and Nafion solution (5%) to form a uniform ink, which is then evenly coated on carbon paper as a working electrode, with Ag / AgCl as a reference electrode, nickel foam as a counter electrode, and 1.0 M KOH as an electrolyte. It is assembled in a flow cell and electrochemically tested by a CHI 760E electrochemical workstation equipped with a CHI 680C current amplifier.

[0026] Sr doping MoSe 2 The powder obtained by ultrasonic exfoliation of mesoporous nanosheet structure material was dispersed into isopropanol and Nafion solution and loaded on carbon paper as cathode, loaded with NiFe 2 O 4 The nickel foam of the NiFe / NiFe LDH was used as the anode and the anolyte was 1.0 M KOH solution. They were assembled in a membrane cell electrolyzer and the electrochemical tests were carried out using a CHI 760E electrochemical workstation equipped with a CHI 680C current amplifier.

[0027] The inventors have found that molybdenum diselenide (MoSe 2 ), a layered VIB disulfide, is a non-toxic and earth-abundant semiconductor material that can be used in CO 2 Theoretical calculations show that MoSe loaded with single atoms (Fe, Co or Ni) has potential application prospects in ER. 2 Nanosheets can react with CO 2 ER showed excellent activity in producing methane. 2 ER products methane and methanol have multiple similar intermediates, and their final products even depend on the last step CH 3 O * The binding strength of the intermediates at the active sites (i.e., active sites with strong affinity to O produce methane, and active sites with moderate affinity to O produce methanol). 2 Electronic structure of nanomaterials to regulate CO 2 The types and proportions of ER products are expected to achieve CO 2 Heteroatom doping can adjust the electronic structure and active sites of the catalyst by hybridizing with the energy level of the original catalyst, thereby regulating CO 2 ER product selectivity.

[0028] The inventors further discovered that the low-valent metal ion Sr 2+ Doping induces electron transfer from Sr to Mo in MoSe 2 Rich selenium vacancies are generated on the lattice, promoting CO 2The adsorption and activation of molecules and their conversion into a series of related C 1 The intermediate generates methanol. The Sr site has a moderate affinity for O atoms, favoring CH 3 O * The intermediate is protonated to methanol. The CO in aqueous solution is effectively overcome in the flow cell of gas diffusion electrode (GDE). 2 The mass transfer limitation caused by low solubility enables methanol production at high current density. 2 ER can effectively alleviate the problems of limited mass transfer, water flooding and high energy consumption in the electrocatalytic process, and achieve CO 2 Therefore, a Sr-doped MoSe 2 Mesoporous nanosheet catalysts can optimize the adsorption behavior of intermediates by regulating their electronic structure and constructing multiple active sites, thus achieving high selectivity, high activity and low energy consumption for electrocatalytic CO catalysis at high current density in flow cells and membrane battery electrolyzers. 2 Reduction to liquid product methanol is of great significance.

[0029] In the preparation method of the present invention, Sr-doped MoSe is synthesized by a one-step chemical liquid phase method. 2 Mesoporous nanosheet structure materials. First, Na dissolved in a mixed solution of water and ethanol 2 MoO 4 ·2H 2 O ionizes MoO 4 2- Ionic groups; hydrazine hydrate (N 2 H 4 ·H 2 O) Under alkaline conditions, Se powder is reduced to Se 2- The role of water is to dissolve Na 2 MoO 4 ·2H 2 O, ethanol plays a role in adjusting the size and thickness of the nanosheets. 2 H 4 ·H 2 O will MoO 4 2- Restore to Mo 4+ .Mo 4+ Further with Se 2- Ion reaction to form hexagonal MoSe 2 Seed crystal, Sr in solution 2+ With MoSe 2 Part of Mo in the lattice 4+ Cation exchange occurs and MoSe is doped 2At the same time, Se vacancies are generated in the lattice to maintain the overall electrical neutrality of the material. Hydrazine hydrate partially decomposes under high temperature conditions to produce N 2 NH 3 , H 2 Gas, filled in MoSe 2 In the process of the seed crystal growing into a nanosheet, it gradually escapes and forms a mesoporous structure on the nanosheet, thus forming Sr 2+ Doped MoSe 2 Mesoporous nanosheet structured materials.

[0030] In the present invention, in MoSe 2 Sr doped into mesoporous nanosheets 2+ Ions can tune MoSe 2 The electronic structure of MoSe 2 Rich selenium vacancies are generated on the lattice. Sr-doped MoSe 2 The positively charged selenium vacancies on the mesoporous nanosheets generate electron-rich regions by extracting electrons from the electrode, which is beneficial for CO 2 molecules and further transform them into curved * CO 2 - Intermediate. Then, * CO 2 - Protonation of intermediates * The COOH intermediate binds to the Mo site adjacent to the Sr site at its C-terminus. Subsequently, it is protonated to form * CO and * CHO intermediate, and further protonated to form CH adsorbed on the Sr site with the O end 2 O * and CH 3 O * Intermediate. The Sr site has a moderate affinity for O, favoring CH 3 O * Protonated to methanol. Due to the low proportion of doped Sr atoms, CH 3 O * The intermediate cannot bind only to the Sr site, and a small amount of CH 3 O * The intermediates adsorb on the Mo sites with strong O affinity, thereby generating methane by breaking the CO bond. In addition, Sr doping enhances the * The adsorption of intermediates can inhibit their desorption from the catalyst surface to form formate. Sr doping stabilizes Mo 4+ site, which can ensure continuous CO 2Electroreduction reaction. At the same time, Sr doping can increase the electrochemical active area of ​​the catalyst, expose more catalytic active sites, improve the conductivity of the catalyst, and significantly increase the transfer rate of interfacial charge. In addition, Sr doping reduces * The free energy barrier for CO generation is conducive to its sequential hydrogenation into methanol products. This material can achieve high selectivity and high current for CO in flow cells and membrane batteries. 2 Electroreduction to methanol. In the flow cell, at a potential of -0.6 V, CO 2 The Faradaic efficiency of ER to methanol is 71.4%, corresponding to a partial current density of 131.7 mA cm -2 After 23 hours of testing, the Faraday efficiency of methanol was 67.3%, and the current density remained at 97.8% of the initial value. In the membrane battery, at a voltage of 3.3 V, the Faraday efficiency of methanol was 68.5%, corresponding to a partial current density of 143.7 mA cm -2 The full cell energy efficiency was 24.9%, and after continuous operation at a voltage of 3.3 V for 42 h, the Faraday efficiency of methanol was 65.3%, and the current density remained at 97.5% of the initial value. 2 It exhibits excellent activity, selectivity and stability in electroreduction and high energy efficiency in membrane cells. 2 The practical application of restoration is very valuable.

[0031] Compared with the prior art, the preparation method of the present invention obtains a thin mesoporous nanosheet structure, which is beneficial to the exposure of the edge active sites and is beneficial to better performance. 2 Sr doping in mesoporous nanosheets 2+ ions can effectively adjust the electronic structure of Sr, Mo and Se atoms, increase the exposure of active sites, form multiple active sites, improve the charge separation efficiency, optimize the intermediate species and their adsorption behavior, and accelerate the catalytic kinetics. 2 Rich selenium vacancies are generated on the lattice, promoting CO 2 The adsorption and activation of molecules and their conversion into a series of related C 1 The intermediate produces methanol. This material can convert CO into CO with high selectivity and high current density in both flow cells and membrane batteries. 2 Electroreduction to methanol liquid product shows excellent activity, selectivity and stability as well as high energy efficiency in membrane batteries. In addition, it has the characteristics of simple preparation process, environmental friendliness and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Sr-doped MoSe prepared in Example 1 2X-ray powder diffraction (XRD) pattern of mesoporous nanosheet structure materials;

[0033] Figure 2 Sr-doped MoSe prepared in Example 1 2 Energy dispersive X-ray (EDX) spectroscopy of mesoporous nanosheet structured materials;

[0034] Figure 3 Sr-doped MoSe prepared in Example 1 2 Scanning electron microscope (SEM) image of mesoporous nanosheet structure material;

[0035] Figure 4 Sr-doped MoSe prepared in Example 1 2 Transmission electron microscopy (TEM) image of mesoporous nanosheet structure material;

[0036] Figure 5 Sr-doped MoSe prepared in Example 1 2 High-resolution transmission electron microscopy (HRTEM) images of mesoporous nanosheet structure materials;

[0037] Figure 6 Sr-doped MoSe prepared in Example 1 2 Scanning transmission electron microscopy (STEM) images of mesoporous nanosheet structure materials and corresponding element distribution maps;

[0038] Figure 7 The Sr-doped MoSe with Sr doping amounts of 2.9% and 8.7% prepared in Example 2 2 X-ray powder diffraction (XRD) pattern of mesoporous nanosheet structure materials;

[0039] Figure 8 The Sr-doped MoSe with Sr doping amounts of 2.9% and 8.7% prepared in Example 2 2 Energy dispersive X-ray (EDX) spectroscopy of mesoporous nanosheet structured materials;

[0040] Fig. 9 The Sr-doped MoSe with a Sr doping amount of 2.9% prepared in Example 2 2 Scanning electron microscope (SEM) image of mesoporous nanosheet structure material;

[0041] Fig.10 The Sr-doped MoSe with a Sr doping amount of 2.9% prepared in Example 2 2 Transmission electron microscopy (TEM) image of mesoporous nanosheet structure material;

[0042] Fig.11 The Sr-doped MoSe with a Sr doping amount of 8.7% prepared in Example 22 Scanning electron microscope (SEM) image of mesoporous nanosheet structure material;

[0043] Fig.12 The Sr-doped MoSe with a Sr doping amount of 8.7% prepared in Example 2 2 Transmission electron microscopy (TEM) image of mesoporous nanosheet structure material;

[0044] Fig.13 Sr-doped MoSe with different Sr doping amounts prepared in Example 1, Example 2 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 LSV curve of mesoporous nanosheet structure material in flow cell;

[0045] Fig.14 Sr-doped MoSe prepared in Example 1 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 Faraday efficiency diagram of mesoporous nanosheet structure materials at different potentials in a flow cell;

[0046] Fig.15 The Sr-doped MoSe with Sr doping amounts of 2.9% and 8.7% prepared in Example 2 2 Faraday efficiency diagram of mesoporous nanosheet structure materials at different potentials in a flow cell;

[0047] Fig.16 The Sr-doped MoSe in Example 1 2 The stability test diagram of the mesoporous nanosheet structure material in the flow cell at a potential of -0.6V for 23h;

[0048] Fig.17 Sr-doped MoSe prepared in Example 1 2 LSV curve of mesoporous nanosheet structure material in membrane battery electrolyzer;

[0049] Fig.18 Sr-doped MoSe prepared in Example 1 2 Faraday efficiency and energy efficiency diagrams of mesoporous nanosheet structure materials at different voltages in membrane battery electrolyzers; solid line I refers to CH 3 The Faradaic efficiency (FE) of the OH product is shown in Figure 1, while the dashed line I refers to the CH 3 Energy efficiency (EE) of OH;

[0050] Fig.19 Sr-doped MoSe prepared in Example 1 2 The stability test diagram of the mesoporous nanosheet structure material in the membrane battery electrolyzer at a voltage of 3.3V for 42 hours;

[0051] Fig. 20 Sr-doped MoSe with different Sr doping amounts prepared in Example 1, Example 2 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 Mesoporous nanosheet structured materials in CO 2 Capacitance-current diagrams at different scan rates under ER conditions;

[0052] Fig.21 Sr-doped MoSe with different Sr doping amounts prepared in Example 1, Example 2 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 Mesoporous nanosheet structured materials in CO 2 Impedance diagram under ER conditions;

[0053] Fig. 22 Sr-doped MoSe with different Sr doping amounts prepared in Example 1, Example 2 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 Mesoporous nanosheet structured materials in CO 2 Hydroxyl groups (OH - ) Adsorption map;

[0054] Fig.23 MoSe prepared in Example 3 2 Mesoporous nanosheet structured materials in CO 2 In-situ diffuse reflectance infrared Fourier transform spectrum of the potential under ER conditions with time at -0.6V;

[0055] Fig.24 Sr-doped MoSe prepared in Example 1 2 Mesoporous nanosheet structured materials in CO 2 In-situ diffuse reflectance infrared Fourier transform spectrum of the potential under ER conditions with time at -0.6V;

[0056] Fig.25 Sr-doped MoSe prepared in Example 1 2 X-ray photoelectron spectroscopy (XPS) diagram of mesoporous nanosheet structure materials;

[0057] Fig.26 X-ray powder diffraction (XRD) patterns of samples prepared with reaction times of 20 h and 28 h in Comparative Example 1 (1);

[0058] Fig. 27 This is a scanning electron microscope (SEM) image of the sample prepared in Comparative Example 1 (1) with a reaction time of 20 h;

[0059] Fig.28This is a scanning electron microscope (SEM) image of the sample prepared in Comparative Example 1 (1) with a reaction time of 28 h;

[0060] Fig.29 The electrocatalytic CO of the sample prepared with a reaction time of 20 h or 28 h in Comparative Example 1 (1) 2 Reduction reaction (CO 2 ER) (the LSV curve of the sample prepared with a reaction time of 24 h in Example 1 is added in the figure as a control).

[0061] Fig.30 This is a scanning electron microscope (SEM) image of the sample prepared at a reaction temperature of 220° C. in Comparative Example 1 (2);

[0062] Fig.31 This is a scanning electron microscope (SEM) image of the sample prepared at a reaction temperature of 260° C. in Comparative Example 1 (2);

[0063] Fig.32 The electrocatalytic CO of the samples prepared at reaction temperatures of 220°C and 260°C in Comparative Example 1 (2) is 2 Reduction reaction (CO 2 ER) (the LSV curve of the sample prepared with a reaction time of 240°C in Example 1 is added in the figure as a control).

[0064] Fig.33 For comparative example 1 (3), the reducing agent is NaBH 4 Scanning electron microscope (SEM) images of the prepared samples;

[0065] Fig.34 For comparative example 1 (3), the reducing agent is NaBH 4 Electrocatalytic CO 2 Reduction reaction (CO 2 ER) (the LSV curve of the sample prepared by adding hydrazine hydrate as the reducing agent in Example 1 is used as a control in the figure);

[0066] Fig.35 The solvent in Comparative Example 1 (4) is 25 mL H 2 Scanning electron microscope (SEM) image of the prepared sample.

[0067] Fig.36 The solvent in Comparative Example 1 (4) is 5 mL H 2 O plus 20 mL of ethanol (C 2 H 5 OH) Scanning electron microscope (SEM) image of the sample prepared;

[0068] Fig.37For Comparative Example 1 (4), the solvent is 25 mL H 2 O or 5 mL HO 2 O plus 20 mL of ethanol (C 2 H 5 Electrocatalytic CO 2 Reduction reaction (CO 2 ER) (the LSV curve of the sample prepared by adding 10 mL of deionized water and 15 mL of ethanol as the solvent in Example 1 is used as a control).

[0069] Fig.38 Ba-doped MoSe prepared in Comparative Example 2 2 X-ray powder diffraction (XRD) pattern of bulk particle structure material;

[0070] Fig.39 Ba-doped MoSe prepared in Comparative Example 2 2 Energy dispersive X-ray (EDX) spectroscopy of bulk granular structured materials;

[0071] Fig.40 Ba-doped MoSe prepared in Comparative Example 2 2 Scanning electron microscope (SEM) images of bulk granular structure materials;

[0072] Fig.41 Ba-doped MoSe prepared in Comparative Example 2 2 LSV curve of bulk granular structure material in flow cell;

[0073] Fig.42 Ba-doped MoSe prepared in Comparative Example 2 2 Faradaic efficiency diagram of the products of bulk granular structure materials at different potentials in a flow cell. DETAILED DESCRIPTION

[0074] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0075] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0076] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0077] Example 1

[0078] The copper foam used in the present invention is treated as follows before use: first, the copper foam (CF) with an area of ​​2×3 cm is immersed in 6M hydrochloric acid for 15 minutes, then washed with deionized water and anhydrous ethanol for 3 times respectively, and dried at room temperature for use.

[0079] Example 1

[0080] A Sr-doped MoSe 2 The preparation method of the mesoporous nanosheet structure material is as follows:

[0081] Weigh 1.0mmol Na 2 MoO 4 ·2H 2 O was added to a mixed solution of 10 mL deionized water and 15 mL anhydrous ethanol and stirred to dissolve. At the same time, 2 mmol of selenium powder was added to 16 mL of 50 wt.% hydrazine hydrate and stirred vigorously for 30 min. The above two solutions were mixed and 0.08 mmol of Sr(NO 3 ) 2 , and stirred vigorously for 30 minutes. Then, the mixed solution and the pre-cleaned copper foam were transferred to a 50 mL polytetrafluoroethylene-lined reactor and reacted in a 240°C oven for 24 hours. After the reaction was completed, the copper foam covering the product was thoroughly washed with deionized water and anhydrous ethanol, first washed with deionized water 3 times, then washed with anhydrous ethanol 3 times, and then dried at 60°C for 6 hours. Sr-doped MoSe 2 Mesoporous nanosheet structured materials.

[0082] Example 1 Structure and morphology characterization of the product:

[0083] The final product obtained in Example 1 was identified by X-ray powder diffractometer (XRD). Figure 1 As shown, it shows that the diffraction peaks of the final product are consistent with the hexagonal MoSe 2 (JCPDS no.72-1420).

[0084] Energy dispersive X-ray (EDX) spectroscopy was used to analyze the composition of the final product. Figure 2 As shown in FIG. 1 , the atomic percentages of Sr, Mo and Se are 0.0635:1:1.8548. According to the atomic ratio of Sr and Mo in the EDX spectrum, the atomic percentage of Sr is calculated to be 6.0% using the formula: x%=Sr / (Sr+Mo)×100%, and the product is defined as Sr 6.0% -MoSe 2 .

[0085] The final product obtained in Example 1 was analyzed by scanning electron microscopy (SEM). Figure 3 As shown, the sample is a uniformly distributed nanosheet structure, the lateral size of the nanosheet is 500-600 nm, and the thickness of the nanosheet is 6-10 nm.

[0086] The transmission electron microscopy (TEM) image of the final product is shown in Figure 4 As shown, it indicates that the sample is a mesoporous nanosheet structure, and the size of the mesopores on the nanosheet is 5 to 36 nm.

[0087] The high resolution transmission electron microscopy (HRTEM) image of the final product is shown in Figure 5 As shown in Figure 2, the nanosheets are further shown to have mesopores (see the two largest circles marked in the lower left figure), where the interplanar spacing of 0.203 nm is similar to that of hexagonal MoSe. 2 The (107) crystal plane matches the nanosheet, and there are a large number of defect structures on the nanosheet (see the small ellipse marked in the lower left figure and the lower right figure).

[0088] The scanning transmission electron microscope element distribution diagram of the final product is shown in Figure 6 As shown, it indicates that Mo, Se and Sr elements are evenly distributed, among which the distribution density of Sr element is relatively low.

[0089] Example 2

[0090] A Sr-doped MoSe 2 The method for preparing a mesoporous nanosheet structure material comprises the following steps:

[0091] Weigh 1.0mmol Na 2 MoO 4 ·2H 2 O was added to a mixed solution of 10 mL of deionized water and 15 mL of anhydrous ethanol and stirred until dissolved. At the same time, 2 mmol of selenium powder was dissolved in 16 mL of 50 wt.% hydrazine hydrate and stirred vigorously for 30 min. The above two solutions were mixed and 0.04 mmol or 0.12 mmol of Sr(NO 3 ) 2 , and stirred vigorously for 30 minutes. Then, the mixed solution and the pre-cleaned copper foam were transferred to a 50 mL polytetrafluoroethylene-lined reactor and reacted in a 240°C oven for 24 hours. After the reaction was completed, the copper foam covering the product was first washed 3 times with deionized water, then washed 3 times with anhydrous ethanol, and then dried at 60°C for 6 hours.

[0092] The product obtained in Example 2 was characterized by X-ray powder diffractometer. Figure 7 All diffraction peaks are consistent with the hexagonal MoSe 2(JCPDS no.72-1420).

[0093] Energy dispersive X-ray spectroscopy (EDX) was used to analyze the composition of the product obtained in Example 2. Figure 8 As shown. It shows that the atomic percentages of Sr, Mo and Se are 0.0295:1:1.8805 and 0.0953:1:1.8134. The doping amount of Sr element is calculated to be 2.9% and 8.7%, and the product is defined as Sr 2.9% -MoSe 2 and Sr 8.7% -MoSe 2 .

[0094] The Sr-doped MoSe with a Sr doping amount of 2.9% prepared in Example 2 was observed using a scanning electron microscope (SEM). 2 The morphology of the mesoporous nanosheet samples was analyzed, such as Fig. 9 As shown, the sample is a nanosheet structure with a lateral size of 500 to 600 nm.

[0095] The Sr-doped MoSe prepared in Example 2 with a Sr doping amount of 2.9% was further examined using a transmission electron microscope (TEM). 2 The morphology of the mesoporous nanosheet samples was analyzed, such as Fig.10 As shown, it indicates that the sample is a mesoporous nanosheet structure, and the size of the mesopores on the nanosheet is 5 to 36 nm.

[0096] The Sr-doped MoSe with a Sr doping amount of 8.7% prepared in Example 2 was observed using a scanning electron microscope (SEM). 2 The morphology of the mesoporous nanosheet samples was analyzed, such as Fig.11 As shown, the sample is a nanosheet structure with a lateral size of 500 to 600 nm.

[0097] The Sr-doped MoSe with a Sr doping amount of 8.7% prepared in Example 2 was further examined using a transmission electron microscope (TEM). 2 The morphology of the mesoporous nanosheet samples was analyzed, such as Fig.12 As shown, it indicates that the sample is a mesoporous nanosheet structure, and the size of the mesopores on the nanosheet is 5 to 36 nm.

[0098] Example 3

[0099] A Sr-doped MoSe 2 Mesoporous nanosheets as electrocatalysts for CO 2 Reduction reaction (CO 2 ER) catalyst, the specific application method is: MoSe 2 Mesoporous nanosheet structure materials or Sr-doped MoSe2 1 mg of mesoporous nanosheet structured material catalyst was dispersed in 0.8 mL of isopropanol and 200 μL of Nafion solution (5%) to form a uniform ink, which was then evenly coated on a carbon paper with a size of 1.0×2.0 cm as a working electrode, with Ag / AgCl as a reference electrode, and a 1.0×2.0 cm nickel foam as a counter electrode. The electrolyte was 1.0 M KOH, assembled in a flow cell, and electrochemical tests were performed using a CHI 760e electrochemical workstation equipped with a CHI 680c current amplifier.

[0100] MoSe 2 The mesoporous nanosheet structure material is obtained by omitting Sr(NO 3 ) 2 Prepared by adding .

[0101] The present invention uses MoSe prepared on foam copper 2 Mesoporous nanosheet structure materials and Sr-doped MoSe 2 Mesoporous nanosheets were used as working electrodes to measure their CO in a gas diffusion electrode flow cell. 2 ER performance and compare them.

[0102] In addition, Sr-doped MoSe 2 0.5 mg of the powder obtained by ultrasonic exfoliation of the mesoporous nanosheet structure material was ultrasonically mixed with 0.8 mL of isopropanol and 200 μL of Nafion solution and loaded on a 1.0 × 1.0 cm carbon paper as the cathode. The 1.0 × 1.0 cm carbon paper was loaded with NiFe 2 O 4 The nickel foam of the NiFe / NiFe LDH was used as the anode and the anolyte was 1.0 M KOH solution. They were assembled in a membrane cell electrolyzer and the electrochemical tests were carried out using a CHI 760e electrochemical workstation equipped with a CHI 680c current amplifier.

[0103] The loads used are NiFe 2 O 4 The preparation method of nickel foam of / NiFe LDH is as follows: take a piece of nickel foam (2×2 cm) and soak it in 6M HCl solution for 15 min, wash it twice with deionized water and anhydrous ethanol; 3 ) 2 , 0.75mmol FeCl 2 and 1.5 mmol NaHCO 3Dissolve in a mixed solvent of 20 mL deionized water and 15 mL methanol and stir for 0.5 h. Then transfer the solution to a 40 mL reactor and place the pre-cleaned nickel foam obliquely and react at 120 ° C for 2 h. After the reaction, wash with deionized water and anhydrous ethanol three times and vacuum dry at 50 ° C for 6 h.

[0104] In the electrochemical test, the linear sweep polarization curve (LSV) was 5.0 mV·s -1 The scan rate was obtained. 2 The Faraday efficiency of ER gas phase products was calculated by gas chromatography (GC2030), and the Faraday efficiency of liquid phase products was calculated by nuclear magnetic resonance hydrogen spectrum ( 1 The stability was obtained by measuring the current density-time curve at a constant potential. -1 Scan rate to obtain OH - Adsorption curves. Electrochemically active surface areas (ECSAs) were calculated by scanning the adsorption rate at different scan rates (10, 20, 30, 40, 50, 60 and 70 mV s -1 ) measure the cyclic voltammogram (CV) and calculate the double layer capacitance (C dl ) was evaluated in the test potential range of -0.05 V to 0.05 V (relative to the reversible hydrogen electrode); the electrochemical impedance spectroscopy (EIS) was obtained at a potential of -0.4 V (relative to the reversible hydrogen electrode) and a frequency range of 100 kHz to 0.01 Hz.

[0105] Fig.13 Sr-doped MoSe with different Sr doping amounts prepared in Example 1, Example 2 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 LSV curve of mesoporous nanosheet structure material in the flow cell. As can be seen from the figure, CO 2 The current density of the LSV polarization curves under the atmosphere is higher than that under the Ar atmosphere, indicating that the samples are more inclined to catalyze CO 2 In the potential range of -0.5 to -1.0 V, the sample with Sr doping content of 6.0% has a strong hydrogen reduction reaction in CO 2 The current density under atmosphere is 129.8~514.8mA·cm -2 , which is higher than that of the sample with Sr doping content of 2.9% (95.4~266.7mA·cm -2 ) and the sample with Sr doping content of 8.7% (108.5~384.3mA·cm -2) and the undoped Sr samples (72.7~213.5mA·cm -2 ). This indicates that Sr doping significantly improves the electrocatalytic CO 2 The reduction reaction activity of Sr was significantly affected by the Sr doping content. 2 As for the reduction reaction activity, the sample with Sr doping amount of 6.0% is more active than those with Sr doping amount of 2.9% and 8.7%.

[0106] Fig.14 Sr-doped MoSe prepared in Example 1 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 Faraday efficiency (FE) diagram of mesoporous nanosheet structure materials at different potentials in the flow cell. It can be seen from the figure that Sr-doped MoSe 2 The Faradaic efficiency of the liquid product methanol reaches 71.4% at -0.6 V, and the Faradaic efficiency of methanol in the potential range of -0.5 to -1.0 V exceeds 45%. 2 The mesoporous nanosheet structure material does not produce liquid product methanol.

[0107] Fig.15 Sr-doped MoSe prepared in Example 2 2 The Faraday efficiency (FE) diagram of mesoporous nanosheet structure materials at different potentials. As can be seen from the figure, the Faraday efficiency of methanol for samples with Sr doping amounts of 2.9% and 8.7% both reached the maximum at -0.6V, which were 62.9% and 67.1% respectively.

[0108] Fig.16 Sr-doped MoSe prepared in Example 1 2 Current density time curve of mesoporous nanosheet structure material in the flow cell at a potential of -0.6 V. According to formula j i =FE×j total , it is calculated that at a potential of -0.6 V, the Sr-doped MoSe prepared in Example 1 2 The partial current density of methanol in mesoporous nanosheet structure material reaches 131.7 mA cm –2 And it can be seen from the figure that Sr doped MoSe 2 After continuous electrolysis of methanol for 23 h at -0.6 V, the Faradaic efficiency of the mesoporous nanosheet structure material was 67.3% and the current density remained at 97.8% of the initial value, indicating that the catalyst has good catalytic stability.

[0109] Fig.17 Sr-doped MoSe prepared in Example 1 2LSV curve of mesoporous nanosheet structure material in membrane battery electrolyzer. It can be concluded from the figure that when the voltage increases from 2.4V to 4.2V, the current density increases from 86.0mA·cm -2 Significantly increased to 368.5 mA cm -2 .

[0110] Fig.18 Sr-doped MoSe prepared in Example 1 2 The Faraday efficiency (FE) and energy efficiency (EE) of mesoporous nanosheet structure materials at different voltages in the membrane battery electrolyzer. It can be seen from the figure that Sr doped MoSe 2 The Faraday efficiency of methanol in the mesoporous nanosheet structure material reaches a maximum of 68.5% at 3.3V, and the energy efficiency reaches a maximum of 24.9%. In addition, liquid product methanol with a Faraday efficiency exceeding 45% can be produced in the voltage range of 2.4V to 4.2V.

[0111] Fig.19 Sr-doped MoSe prepared in Example 1 2 Current density time curve of mesoporous nanosheet structure material in membrane battery electrolyzer at voltage of 3.3V. According to formula j i =FE×j total , the Sr-doped MoSe prepared in Example 1 is calculated 2 The partial current density of methanol in mesoporous nanosheet structure material reaches 143.7 mA cm –2 And it can be seen from the figure that after continuous electrolysis of methanol at a voltage of 3.3V for 42h, the Faradaic efficiency of methanol can still reach 65.3%, and the current density remains at 97.5% of the initial value, indicating that the material has good catalytic stability in the membrane battery electrolyzer.

[0112] Fig. 20 Sr-doped MoSe with different Sr doping amounts prepared in Example 1, Example 2 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 Mesoporous nanosheet structure material CO 2 Capacitance-current diagrams at different scan rates under ER conditions. The double-layer capacitance of the sample with a Sr doping content of 6.0% is 20.43 mF·cm -2 , which is greater than that of the sample with Sr doping content of 2.9% (16.73 mF·cm -2 ), the sample with Sr doping content of 8.7% (17.61mF·cm -2 ), which are much larger than those of the sample without Sr doping (8.91 mF·cm -2). This indicates that Sr doping increases the electrochemical active area of ​​the sample, and the sample with a Sr doping amount of 6.0% has the largest electrochemical active area.

[0113] Fig.21 Sr-doped MoSe with different Sr doping amounts prepared in Example 1, Example 2 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 Mesoporous nanosheet structured materials in CO 2 Electrochemical impedance spectroscopy (EIS) graph under ER conditions. The charge transfer resistance (R ct ) is 44.07Ω, which is less than the sample with Sr doping amount of 2.9% (61.80Ω) and the sample with Sr doping amount of 8.7% (54.25Ω), while the charge transfer resistance of the sample without Sr doping is the largest (75.98Ω). This shows that Sr doping increases the conductivity of the sample. 2 Mesoporous nanosheets have the lowest electrical resistance and the fastest catalytic kinetics.

[0114] Fig. 22 Sr-doped MoSe with different Sr doping amounts prepared in Example 1, Example 2 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 The hydroxyl groups (OH - ) adsorption diagram. * CO 2 - The binding strength on the catalyst surface is related to OH - Positive correlation between adsorption and OH - Adsorption strength was evaluated * CO 2 - The bonding strength on the catalyst surface. As shown in the figure, the OH of samples with Sr doping amounts of 2.9%, 6.0% and 8.7% - The adsorption potentials are -0.29 V, -0.44 V and -0.37 V respectively, while the OH of the undoped Sr sample - The adsorption potential is -0.21 V. This indicates that Sr doped MoSe 2 OH on mesoporous nanosheets - The adsorption potential is lower than that of the sample without Sr doping, and the OH - The adsorption potential is the most negative, so its adsorption to OH - The strongest affinity can effectively stabilize * CO 2 - Intermediate, accelerating CO 2ER process.

[0115] Fig.23 Undoped MoSe prepared in Example 3 2 Mesoporous nanosheet structured materials in CO 2 In-situ diffuse reflectance infrared Fourier transform spectrum obtained by testing every 1 minute at -0.6V potential under ER conditions. As can be seen from the figure, with the increase of electrolysis time, * CO 2 - The peak intensity of CO gradually increased until 13 min later, when it remained unchanged, indicating that its coverage on the catalyst increased. 2 Adsorption increases and can be converted into more * CO 2 - Intermediates can provide more reactants for subsequent reactions. * The CO vibration peak intensity of the COOH intermediate gradually increases with time, indicating that its coverage on the catalyst surface increases, which is conducive to further conversion to * CO B Intermediate. * CO B The intensity of the intermediate peak gradually increased with time and was accompanied by a red shift, indicating that its coverage on the catalyst surface increased but the adsorption intensity weakened, thereby inhibiting the CO 2 The deep restoration of * CO B Easily desorbs from active sites to form CO. HCOO * The peak intensity of the intermediate gradually increases with time, indicating that its coverage on the catalyst surface increases, thereby promoting the formation of formate. 2 O * The peak intensity of the intermediate gradually increases with time, indicating that it is conducive to the formation of methane. In addition, with the increase of electrolysis time, * The peak intensity of the OH peak increases, indicating that the coverage of water molecules on the catalyst surface increases, which can dissociate more protons for HCOO * The intermediate is protonated to formate.

[0116] Fig.24 Sr-doped MoSe prepared in Example 1 2 Mesoporous nanosheet structured materials in CO 2 The in-situ diffuse reflectance infrared Fourier transform spectrum obtained by testing every 1 minute under ER conditions at a potential of -0.6 V. As can be seen from the figure, as the electrolysis time increases, The peak intensity gradually

[0117] increased until 13 min later, when it remained constant, indicating that its coverage on the catalyst increased, thus CO 2 Increased adsorption can provide more reactants for subsequent reactions. * The CO vibration peak intensity of the COOH intermediate increases, accompanied by a gradual blue shift and the appearance of a new * The OH deformation vibration peak of the COOH intermediate indicates that its coverage on the catalyst surface is increased and its adsorption is enhanced, which is conducive to its further conversion into a bridge-type with high coverage. * CO B , which is used for subsequent reactions and also forms a linear * CO L , three-site or multi-site adsorption * CO T or * CO M Intermediate. High coverage * CO B After continuous hydrogenation, it can be converted into more * CHO, CH 2 O * and CH 3 O * Finally, CH 3 O * Further hydrogenation produces methanol. * The peak position of OH gradually blue-shifted and was accompanied by an increase in peak intensity, indicating that the intensity of water molecules adsorbed on the catalyst surface increased and the coverage increased, indicating that more protons can be dissociated for the protonation of carbon intermediates.

[0118] Fig.25 Sr-doped MoSe prepared in Example 1 and Example 3 2 Mesoporous nanosheet structure materials and MoSe 2 X-ray photoelectron spectroscopy (XPS) of mesoporous nanosheet structure materials. 2 In comparison, Sr 6.0% -MoSe 2 The Mo 3d peak position in the quartz crystal shifted negatively, while the Se 3d peak position remained unchanged. This is because the electronegativity of Mo (2.16) is higher than that of Sr (0.95), resulting in electron transfer from Sr to Mo. This shows that doping Sr can effectively optimize the MoSe 2 electronic structure to improve the charge separation efficiency.

[0119] The present invention utilizes a one-step liquid phase method to construct Sr 2+ Doped MoSe 2 Mesoporous nanosheets can effectively optimize the electronic structure of the catalyst and form multiple active sites. 2+Doping results in electron transfer from Sr to Mo and induces the creation of Se vacancies, which makes the Sr site show a moderate affinity for O and favors CH 3 O * The key intermediate is protonated to methanol. At the same time, Sr doping can increase the electrochemical active area of ​​the catalyst and expose more catalytic active sites. In addition, Sr doping improves the conductivity of the catalyst, significantly increases the transfer rate of interfacial charge, and accelerates catalytic kinetics. 2 Mesoporous nanosheet-structured materials in electrocatalytic CO 2 The application of methanol electrocatalyst materials for reducing to liquid product has the characteristics of low overpotential at high current density, high selectivity, good stability, high energy efficiency, simple preparation process and environmental friendliness. 2 The practical application of restoration is very valuable.

[0120] Comparative Example 1

[0121] According to Example 1, Sr-doped MoSe 2 The preparation method of mesoporous nanosheet structure is carried out in the same way, the difference lies only in the control of the following parameters:

[0122] (1) The preparation method was the same as in Example 1, except that the reaction time was different: the solvent thermal reaction time was kept at 20 h or 28 h, respectively, and the other variables remained the same.

[0123] (2) The preparation method is the same as in Example 1, except that the reaction temperature is kept at 220°C or 260°C, respectively, and the other variables remain the same.

[0124] (3) The preparation method is the same as in Example 1, except that the reducing agent is changed to NaBH 4 (10 mmol), and the other variables remained the same.

[0125] (4) The preparation method was the same as in Example 1, except that the solvent was changed to 25 mL H 2 O or 5 mL HO 2 O was added with 20 mL of ethanol, and the other variables remained the same.

[0126] Fig.26 The X-ray powder diffraction (XRD) patterns of the samples prepared by the solvent thermal reaction for 20 h or 28 h in Comparative Example 1 (1). When the reaction time is 20 h, except for MoSe 2 In addition to the diffraction peaks of MoO 2 The diffraction peaks of MoSe 2 diffraction peaks.

[0127] Fig. 27This is a scanning electron microscope (SEM) image of the sample prepared by solvothermal reaction for 20 hours in Comparative Example 1 (1), indicating that the sample is an incompletely grown nanosheet structure.

[0128] Fig.28 This is a scanning electron microscope (SEM) image of the sample prepared by solvothermal reaction for 28 hours in Comparative Example 1 (1). As can be seen from the image, the obtained sample is a thick nanosheet structure, and particles with an average size of 80 nm are unevenly attached to the surface and edge of the nanosheet.

[0129] Fig.29 The electrocatalytic CO of the sample prepared by the solvent thermal reaction time of 20 h or 28 h in Comparative Example 1 (1) is 2 Reduction reaction (CO 2 The LSV curve of the sample prepared with a reaction time of 24 h in Example 1 is added as a control. As can be seen from the figure, the current density of the sample with a reaction time of 20 h in the potential range of -0.5 V to -1.0 V is 61.1 mA·cm -2 ~220.8mA·cm -2 The current density of the sample with a reaction time of 28 h in the potential range of -0.5 V to -1.0 V is 87.1 mA·cm -2 ~381.4mA·cm -2 . It shows that the synthesis of Sr-doped MoSe 2 The reaction time of mesoporous nanosheets significantly affects the electrocatalytic CO 2 Reduction reaction (CO 2 ER) activity, the sample with a reaction time of 24 h electrocatalyzed CO 2 Reduction reaction (CO 2 The ER) activity was better than that of the samples with reaction time of 20h and 28h.

[0130] Fig.30 This is a scanning electron microscope (SEM) image of the sample prepared at a reaction temperature of 220° C. in Comparative Example 1 (2). As can be seen from the image, the sample is an incompletely grown nanosheet structure.

[0131] Fig.31 This is a scanning electron microscope (SEM) image of the sample prepared at a reaction temperature of 260° C. in Comparative Example 1 (2). As can be seen from the image, the sample is a nanosheet structure with uneven thickness, and the average lateral size of the nanosheet is about 400 nm.

[0132] Fig.32 The electrocatalytic CO of the samples prepared at reaction temperatures of 220°C and 260°C in Comparative Example 1 (2) is 2 Reduction reaction (CO 2The LSV curve of the sample prepared at a reaction temperature of 240°C in Example 1 is added as a control. As can be seen from the figure, the current density of the sample prepared at a reaction temperature of 220°C in the potential range of -0.5V to -1.0V is 53.3mA·cm -2 ~263.6mA·cm -2 The current density of the sample with a reaction temperature of 260°C in the potential range of -0.5V to -1.0V is 73.2mA·cm -2 ~344.6mA·cm -2 , indicating that the synthesis of Sr-doped MoSe 2 The reaction temperature of nanostructured materials significantly affects the electrocatalytic CO 2 Reduction reaction (CO 2 ER) activity, the sample with reaction temperature of 240℃ electrocatalyzed CO 2 Reduction reaction (CO 2 The ER) activity was better than that of the samples with reaction temperatures of 220℃ and 260℃.

[0133] Fig.33 For comparative example 1 (3), the reducing agent is NaBH 4 Scanning electron microscope (SEM) image of the prepared sample. As can be seen from the image, the sample is a randomly stacked, unevenly sized and unevenly thick nanosheet structure.

[0134] Fig.34 For comparative example 1 (3), the reducing agent is NaBH 4 Electrocatalytic CO 2 Reduction reaction (CO 2 The LSV curve of the sample prepared by adding hydrazine hydrate as the reducing agent in Example 1 is shown in the figure as a control. 4 The current density of the sample in the potential range of -0.5V to -1.0V is 53.1mA·cm -2 ~320.2mA·cm -2 , indicating that the synthesis of Sr-doped MoSe 2 The reductant of the nanostructured material significantly affects the morphology of the sample and further affects the electrocatalytic CO 2 Reduction reaction (CO 2 ER) activity.

[0135] Fig.35 The solvent in Comparative Example 1 (4) is 25 mL H 2 Scanning electron microscope (SEM) image of the sample prepared by O. As can be seen from the figure, the sample is still a nanosheet structure, but the size of the nanosheet becomes larger and thicker, with a lateral size of 600-1000nm and a thickness of 20-50nm.

[0136] Fig.36 The solvent in Comparative Example 1 (4) is 5 mL H 2 O plus 20 mL of ethanol (C 2 H 5 Scanning electron microscope (SEM) image of the sample prepared by OH). As can be seen from the image, the sample presents a very small nanosheet structure with a lateral size of 100 to 300 nm.

[0137] Fig.37 For Comparative Example 1 (4), the solvent is 25 mL H 2 O or 5 mL HO 2 O plus 20 mL of ethanol (C 2 H 5 OH) prepared samples were used for electrocatalysis of CO 2 Reduction reaction (CO 2 The LSV curve of the sample prepared by adding 10 mL of deionized water and 15 mL of anhydrous ethanol as the solvent of Example 1 is shown in the figure as a control. 2 The current density of the sample with O in the potential range of -0.5V to -1.0V is 76.9mA·cm -2 ~322.2mA·cm -2 The results showed that larger and thicker nanosheets exposed fewer active sites, resulting in lower catalytic activity. The solvent was 5 mL H 2 O plus 20 mL of ethanol (C 2 H 5 The current density of the sample containing OH) in the potential range of -0.5V to -1.0V is 34.2mA·cm -2 ~241.5mA·cm -2 The results show that too small nanosheets will cause nanosheets to agglomerate due to excessive surface energy during the catalytic process, which will reduce the catalytic performance. This shows that the solvent will affect the Sr-doped MoSe 2 The morphology of nanostructured materials further affects the electrocatalytic CO 2 Reduction reaction (CO 2 ER) activity.

[0138] Comparative Example 2

[0139] A Ba-doped MoSe 2 The preparation method of the blocky particle structure material is as follows:

[0140] Weigh 1.0mmol Na 2 MoO 4 ·2H 2O was added to a mixed solution of 10 mL of deionized water and 15 mL of anhydrous ethanol and stirred to dissolve. At the same time, 2 mmol of selenium powder was added to 16 mL of 50 wt.% hydrazine hydrate and stirred vigorously for 30 min. The above two solutions were mixed and 0.08 mmol of Ba(NO 3 ) 2 , and stirred vigorously for 30 minutes. Then, the mixed solution and the pre-cleaned copper foam were transferred to a 50 mL polytetrafluoroethylene-lined reactor and reacted in a 240°C oven for 24 hours. After the reaction was completed, the copper foam covering the product was washed 3 times with deionized water, then washed 3 times with anhydrous ethanol, and then dried at 60°C for 6 hours. Ba-doped MoSe 2 Blocky granular structure material.

[0141] Fig.38 Ba-doped MoSe prepared in Comparative Example 2 2 X-ray powder diffraction (XRD) pattern of bulk granular structure materials. Ba-doped MoSe 2 The diffraction peaks of bulk granular structure materials are similar to those of hexagonal MoSe 2 (JCPDS no.72-1420).

[0142] Fig.39 Ba-doped MoSe prepared in Comparative Example 2 2 Energy dispersive X-ray (EDX) spectra of bulk granular structure materials. As shown in the figure, Ba-doped MoSe 2 The energy dispersive X-ray (EDX) spectrum of the bulk particles showed a peak of Ba, indicating that Ba was successfully doped into MoSe. 2 The atomic percentages of Ba, Mo and Se in the EDX spectrum are 0.0629:1:1.8610. The atomic percentage of Ba is 5.9% calculated using the formula: x%=Ba / (Ba+Mo)×100%. The product is defined as Ba 5.9% -MoSe 2 .

[0143] Fig.40 The Ba-doped MoSe prepared in Comparative Example 2 2 Scanning electron microscope (SEM) image of bulk particle structure material. As can be seen from the image, the sample is a block of particles with uneven sizes, ranging from 40nm to 500nm.

[0144] Fig.41 Ba-doped MoSe prepared in Comparative Example 2 2 LSV curve of bulk granular structure materials in a flow cell. Ba-doped MoSe 2 Blocky granular structure materials in CO 2When the potential range is -0.5V to -1.0V under the atmosphere, the current density is 82.5mA·cm -2 ~224.9mA·cm -2 , which is smaller than Sr-doped MoSe under the same potential range. 2 The current density of the sample prepared by the mesoporous nanosheet structure material. It shows that the CO 2 ER performance is lower than that of Sr-doped MoSe 2 Samples prepared from mesoporous nanosheet structured materials.

[0145] Fig.42 Ba-doped MoSe prepared in Comparative Example 2 2 Faraday efficiency (FE) diagram of bulk granular structure materials at different potentials in the flow cell. It can be seen from the figure that Ba-doped MoSe 2 The products are formate, methane, carbon monoxide and hydrogen, and no liquid product methanol is produced. In addition, the FE of formate, methane and carbon monoxide are all smaller than that of undoped MoSe 2 , indicating that Ba doping does not bring CO 2 The results show that Sr doped MoSe 2 Mesoporous nanosheet structure materials have excellent CO 2 The ER performance and the generation of methanol product are caused by Sr doping.

[0146] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for preparing Sr-doped molybdenum diselenide mesoporous nanosheet structure material, characterized in that: The preparation method is: A molybdenum source is placed in a mixed solvent of water and ethanol, and a selenium source is placed in a reducing agent solution. After the two solutions are mixed, a strontium source is added, and foam copper is placed in the solution to carry out a solvothermal reaction to obtain an Sr-doped molybdenum diselenide mesoporous nanosheet structure material.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the strontium source, the molybdenum source and the selenium source is 0.04-0.12:1:

2.

3. The preparation method according to claim 1 or 2, characterized in that: The usage ratio of the molybdenum source to water is 0.1 mol / L.

4. The preparation method according to claim 1, characterized in that: The strontium source is selected from soluble strontium salts, the molybdenum source is a soluble molybdenum salt, and the selenium source is selenium powder.

5. The preparation method according to claim 1, characterized in that: The reducing agent solution is a hydrazine hydrate aqueous solution with a mass fraction of 50 wt.%.

6. The preparation method according to claim 1 or 5, characterized in that: The volume ratio of the ethanol, water and reducing agent is 7.5-22.5:5-15:8-24.

7. The preparation method according to claim 1 or 5, characterized in that: The solvent thermal reaction is carried out at 230-250° C. for 23-25 ​​hours.

8. A Sr-doped molybdenum diselenide mesoporous nanosheet structure material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The morphology of the Sr-doped molybdenum diselenide mesoporous nanosheet structure material is a mesoporous nanosheet structure material in which mesopores with a size of 5 to 36 nm are distributed on nanosheets with a lateral size of 500 to 600 nm and a thickness of 6 to 10 nm.

9. An application of the Sr-doped molybdenum diselenide mesoporous nanosheet structure material according to claim 8, characterized in that: The Sr-doped molybdenum diselenide mesoporous nanosheet structure material is used as an electrocatalyst for electrocatalytic carbon dioxide reduction reaction.

10. The use according to claim 9, characterized in that: The Sr-doped molybdenum diselenide mesoporous nanosheet structure material is used as an electrocatalyst for electrocatalytic carbon dioxide reduction reaction to produce methanol.