Preparation method of wormlike MgO / Mo2C / NC electrolyzed water hydrogen production catalyst

Through the preparation of worm-like MgO/Mo2C/NC electrolytic hydrogen production catalyst, the problem of insufficient activity and stability of Mo2C-based electrocatalysts is solved, the electrocatalytic HER performance is improved, and the electrocatalytic HER design idea is provided.

CN118932394APending Publication Date: 2024-11-12SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410986107.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing Mo2C-based electrocatalysts have low catalytic activity and poor stability during electrochemical water decomposition, resulting in low energy conversion efficiency of electrolytic water.

Method used

The preparation method of worm-like MgO/Mo2C/NC electrolytic hydrogen production catalyst is adopted, and the MgO/Mo2C/NC structure is constructed through ultrasonic dispersion, stirring and sintering processes, and the electronic structure and interface characteristics are optimized, and the catalytic activity and stability are improved.

Benefits of technology

It has achieved significant improvements in catalytic activity and stability, improved electrocatalytic HER performance, simple process and mild conditions, and is suitable for heterostructure electrocatalyst design in other fields of electrocatalytic and energy conversion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932394A_ABST
    Figure CN118932394A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a wormlike MgO / Mo2C / NC electrolytic water hydrogen production catalyst, which comprises the following steps: step 1, firstly weighing 0.095-0.3 g of magnesium source and 0.1-3 g of molybdenum source, putting into a beaker, then adding 20-80 mL of absolute ethyl alcohol into the beaker, and then sequentially carrying out ultrasonic dispersion, stirring and drying to obtain colorless powder; and 2, mixing the colorless powder obtained in the step 1 with 0.5-3 g of a carbon source, grinding, fully and uniformly mixing, putting into a porcelain boat, putting the porcelain boat into a tubular furnace, introducing argon gas into the tubular furnace, heating from room temperature to 750-850 DEG C at a heating rate of 5-10 DEG C / min, keeping the temperature for 1-3 hours, cooling to room temperature after the reaction is finished, and grinding to obtain the black powdery wormlike MgO / Mo2C / NC electrolytic water hydrogen production catalyst, the catalyst has excellent catalytic activity and stability, and can improve the electro-catalysis HER performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochemical water decomposition hydrogen production, and specifically is a method for preparing a worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst. Background Art

[0002] Finding clean energy is crucial for the sustainable development of society. Hydrogen is a good alternative to traditional fossil fuels. In practice, hydrogen can be efficiently and sustainably produced by electrochemical decomposition of water. Highly active electrocatalysts are needed to accelerate the hydrogen evolution reaction, such as precious metals Pt, Pd, Ru and Au, which are considered to be the most effective and stable HER electrocatalysts due to their excellent hydrogen bonding energy and almost zero initial overpotential, but their high cost hinders their widespread use.

[0003] Transition metal molybdenum carbide (Mo2C) is a promising electrocatalyst with an electronic structure similar to that of Pt due to the hybridization of the d orbital of the molybdenum atom with the s and p orbitals of carbon. In recent years, the hydrogen evolution performance of Mo2C has been optimized by adopting heteroatom doping, heterointerface design and surface defect construction strategies, and has played a positive role; however, the existing Mo2C-based catalysts still have the problems of low catalytic activity and poor stability in the process of electrochemical water decomposition, which makes the energy conversion efficiency of water electrolysis too low. Therefore, how to further optimize the hydrogen evolution performance of Mo2C remains an important task. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst, and the prepared MgO / Mo2C / NC water electrolysis hydrogen production catalyst has excellent catalytic activity and stability.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst comprises the following steps:

[0007] Step 1, weigh 0.095-0.3 g of magnesium source and 0.1-3 g of molybdenum source into a beaker, then add 20-80 mL of anhydrous ethanol to the beaker, and then ultrasonically disperse, stir and dry in sequence to obtain a colorless powder;

[0008] Step 2: Mix the colorless powder obtained in step 1 with 0.5-3 g of a carbon source, grind them to make them fully mixed, and then put them into a porcelain boat. The porcelain boat is placed in a tubular furnace, and argon gas is introduced into the tubular furnace. The temperature is increased from room temperature to 750-850° C. at a heating rate of 5-10° C. / min, and the temperature is kept for 1-3 hours. After the reaction is completed, the mixture is cooled to room temperature and ground to obtain a black powdery worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst.

[0009] Furthermore, the magnesium source in step 1 is magnesium chloride, magnesium chlorate or magnesium nitrate.

[0010] Furthermore, the molybdenum source in step 1 is molybdenum trioxide, molybdenum chloride or ammonium molybdate.

[0011] Furthermore, the ultrasonic dispersion time in step 1 is 20 to 60 minutes.

[0012] Furthermore, the stirring in step 1 is performed using a magnetic stirrer at a speed of 400 to 600 r / min for 10 to 40 min.

[0013] Furthermore, the drying in step 1 is carried out in an oven at 50-80° C. for 5-6 hours.

[0014] Furthermore, the carbon source in step 2 is dicyandiamide, melamine or glucose.

[0015] Furthermore, the grinding time in step 2 is 3 to 5 minutes.

[0016] Compared with the prior art, the present invention has the following technical effects:

[0017] The present invention constructs a MgO / Mo2C / NC structure through a simple one-step sintering process. On the one hand, the electronic structure of the heterojunction electrocatalyst is optimized through the interaction between charges, so that the electrons around Mo are rearranged and the Mo-H binding energy is weakened, that is, the hydrogen adsorption free energy is adjusted, and the hydrogen adsorption and precipitation process is accelerated. At the same time, the rich high-activity interface has a low charge transfer resistance and can promote electrolyte diffusion, thereby improving the activity of the catalyst; on the other hand, the rich carbon base load improves the conductivity of the catalyst, accelerates charge transfer and separation, and effectively accelerates the reaction kinetic energy mass transfer. The worm-like structure increases the active catalytic sites, is easy to contact with the reactive substances, and improves the catalyst structure stability; in short, the worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst prepared by the present invention has excellent catalytic activity and stability, and can improve the electrocatalytic HER performance.

[0018] The preparation method of the present invention has the advantages of simple process, mild reaction conditions, high operability and easy process control, and can be extended to the preparation of other heterogeneous structure electrocatalysts used for electrocatalysis and energy conversion, providing a new idea for the design and construction of efficient and durable electrocatalysts in the field of energy storage and conversion. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The RXD spectrum of the worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst prepared in Example 1 of the present invention;

[0020] Figure 2 This is a SEM image of the worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst prepared in Example 1 of the present invention;

[0021] Figure 3 This is the LSV diagram of the worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.

[0023] Example 1

[0024] Step 1, first weigh 0.095g magnesium chloride and 0.5g molybdenum trioxide into a beaker, then add 50mL of anhydrous ethanol to the beaker, ultrasonically disperse for 30min to form a suspension, then place the beaker containing the suspension on a magnetic stirrer, stir at a speed of 500r / min for 10min, to obtain solution A;

[0025] Step 2, place the beaker containing solution A in a drying oven at 60°C and dry for 6 hours to obtain colorless powder B;

[0026] Step 3: Mix the colorless powder B obtained in step 1 with 1.0 g of melamine, grind for 3 minutes to fully mix, then load into a porcelain boat, put the porcelain boat into a tubular furnace, introduce argon into the tubular furnace, and heat from room temperature to 750°C at a heating rate of 5°C / min. Keep warm for 2 hours. After the reaction is completed, cool to room temperature, take out the product and grind it to obtain a black powdery worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst.

[0027] from Figure 1 It can be seen that the characteristic diffraction peaks are located at 34.4°, 37.9° and 39.4°, respectively, corresponding to the (100), (002) and (101) crystal planes of typical β-Mo2C. In addition, there is a weak diffraction peak of MgO, and no other impurity peaks appear, which proves that Example 1 successfully prepared the MgO / Mo2C / NC water electrolysis hydrogen production catalyst.

[0028] from Figure 2 It can be seen that the main morphology of the sample is worm-like distribution on the substrate. The special morphology exposes more active sites on the catalyst surface and has a larger specific surface area, which can accelerate the diffusion of reactants and is beneficial to improving the performance of the catalyst. In addition, active reaction substances are easier to adhere, which reduces the activation energy in the electrochemical reaction and exhibits good catalytic activity.

[0029] from Figure 3 It can be seen that the synthesized non-precious metal MgO / Mo2C / NC by a simple one-step sintering method has a high conductivity at 10 mA / cm2 in 1 M KOH electrolyte. 2 The overpotential at a current density of 111 mV is shown, showing excellent hydrogen evolution activity, thus providing a novel approach for the design of high-performance non-precious metal catalysts for HER.

[0030] Example 2

[0031] Step 1, first weigh 0.143g of magnesium chlorate and 0.1g of ammonium molybdate into a beaker, then add 20mL of anhydrous ethanol into the beaker, and ultrasonically disperse for 20min to form a suspension, then place the beaker containing the suspension on a magnetic stirrer, and stir at a speed of 400r / min for 40min to obtain solution A;

[0032] Step 2, place the beaker containing solution A in a drying oven at 50°C and dry for 6 hours to obtain colorless powder B;

[0033] Step 3: Mix the colorless powder B obtained in step 1 with 0.5 g of dicyandiamide, grind for 4 minutes to fully mix them, then load them into a porcelain boat, put the porcelain boat into a tubular furnace, introduce argon into the tubular furnace, and heat from room temperature to 800°C at a heating rate of 5°C / min. Keep warm for 2 hours. After the reaction is completed, cool to room temperature, take out the product and grind it to obtain a black powdery worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst.

[0034] Example 3

[0035] Step 1, first weigh 0.25g of magnesium chlorate and 1.5g of molybdenum chloride into a beaker, then add 30mL of anhydrous ethanol to the beaker, ultrasonically disperse for 40min to form a suspension, then place the beaker containing the suspension on a magnetic stirrer, stir at a speed of 550r / min for 20min, to obtain solution A;

[0036] Step 2, place the beaker containing solution A in a drying oven at 70°C and dry for 6 hours to obtain colorless powder B;

[0037] Step 3: Mix the colorless powder B obtained in step 1 with 3.0 g of melamine, grind for 5 minutes to fully mix them, then put them into a porcelain boat, put the porcelain boat into a tubular furnace, introduce argon into the tubular furnace, and heat from room temperature to 800°C at a heating rate of 8°C / min. Keep warm for 3 hours. After the reaction is completed, cool to room temperature, take out the product and grind it to obtain a black powdery worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst.

[0038] Example 4

[0039] Step 1, first weigh 0.19g magnesium nitrate and 2g molybdenum chloride into a beaker, then add 60mL anhydrous ethanol to the beaker, ultrasonically disperse for 50min to form a suspension, then place the beaker containing the suspension on a magnetic stirrer, stir at a speed of 550r / min for 30min, to obtain solution A;

[0040] Step 2, place the beaker containing solution A in a drying oven at 80°C and dry for 5 hours to obtain colorless powder B;

[0041] Step 3: Mix the colorless powder B obtained in step 1 with 2.0 g of dicyandiamide, grind for 5 minutes to fully mix them, then load them into a porcelain boat, put the porcelain boat into a tubular furnace, introduce argon into the tubular furnace, and heat from room temperature to 850°C at a heating rate of 10°C / min. Keep warm for 1 hour. After the reaction is completed, cool to room temperature, take out the product and grind it to obtain a black powdery worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst.

[0042] Example 5

[0043] Step 1, first weigh 0.3g magnesium nitrate and 3g ammonium molybdate into a beaker, then add 80mL anhydrous ethanol into the beaker, ultrasonically disperse for 60min to form a suspension, then place the beaker containing the suspension on a magnetic stirrer, stir at a speed of 600r / min for 20min to obtain solution A;

[0044] Step 2, place the beaker containing solution A in a drying oven at 60°C and dry for 5 hours to obtain colorless powder B;

[0045] Step 3: Mix the colorless powder B obtained in step 1 with 1.5 g of glucose, grind for 5 minutes to fully mix, then load into a porcelain boat, put the porcelain boat into a tubular furnace, introduce argon into the tubular furnace, and heat from room temperature to 800° C. at a heating rate of 10° C. / min. Keep warm for 2 hours. After the reaction is completed, cool to room temperature, take out the product and grind it to obtain a black powdery worm-like MgO / Mo2C / NC water electrolysis hydrogen production catalyst.

Claims

1. A worm-like MgO / Mo 2 Preparation method of C / NC water electrolysis hydrogen production catalyst, It is characterized in that The steps include: Step 1, weigh 0.095-0.3 g of magnesium source and 0.1-3 g of molybdenum source into a beaker, then add 20-80 mL of anhydrous ethanol to the beaker, and then ultrasonically disperse, stir and dry in sequence to obtain a colorless powder; Step 2: Mix the colorless powder obtained in step 1 with 0.5-3g of carbon source, grind, mix thoroughly and evenly, put into a porcelain boat, put the porcelain boat into a tube furnace, introduce argon gas into the tube furnace, heat from room temperature to 750-850°C at a heating rate of 5-10°C / min, keep warm for 1-3h, cool to room temperature after the reaction is completed, grind, and obtain black powdery worm-like MgO / Mo 2 C / NC catalyst for hydrogen production from water electrolysis.

2. The worm-like MgO / Mo according to claim 1 2 Preparation method of C / NC water electrolysis hydrogen production catalyst, It is characterized in that The magnesium source in step 1 is magnesium chloride, magnesium chlorate or magnesium nitrate.

3. The worm-like MgO / Mo according to claim 1 2 Preparation method of C / NC water electrolysis hydrogen production catalyst, It is characterized in that The molybdenum source in step 1 is molybdenum trioxide, molybdenum chloride or ammonium molybdate.

4. The worm-like MgO / Mo according to claim 1 2 Preparation method of C / NC water electrolysis hydrogen production catalyst, It is characterized in that The ultrasonic dispersion time in step 1 is 20 to 60 minutes.

5. The worm-like MgO / Mo according to claim 1 2 Preparation method of C / NC water electrolysis hydrogen production catalyst, It is characterized in that The stirring in step 1 is performed by using a magnetic stirrer at a speed of 400 to 600 r / min for 10 to 40 minutes.

6. The worm-like MgO / Mo according to claim 1 2 Preparation method of C / NC water electrolysis hydrogen production catalyst, It is characterized in that The drying in step 1 is performed in an oven at 50-80° C. for 5-6 hours.

7. The worm-like MgO / Mo according to claim 1 2 Preparation method of C / NC water electrolysis hydrogen production catalyst, It is characterized in that The carbon source in step 2 is dicyandiamide, melamine or glucose.

8. The worm-like MgO / Mo according to claim 1 2 Preparation method of C / NC water electrolysis hydrogen production catalyst, It is characterized in that The grinding time of step 2 is 3 to 5 minutes.