Membrane electrode assembly and water electrolysis device

By using a solid polymer electrolyte membrane of a woven fabric composed of fluoropolymer and a specified denier number in the water electrolytic device, the problems of insufficient strength and high electrolytic voltage are solved, and excellent strength and electrolytic voltage are achieved. Reduced effect.

CN118932412APending Publication Date: 2024-11-12AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118052.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-02-08
Filing Date
2020-02-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The membrane electrode joint used in the existing water electrolytic device has insufficient strength under pressure and has a high electrolytic voltage, making it difficult to take into account both the strength and the electrolytic voltage.

Method used

A solid polymer electrolyte film containing a fluorine-containing polymer and a woven fabric consisting of a specified denier number is used to satisfy specific relationships by adjusting the opening rate of the woven fabric, the denier number of yarn, the film thickness and the ion exchange capacity. Formula Y≤240X-170 is used to increase the strength of the membrane electrode joint and reduce the electrolytic voltage.

Benefits of technology

In the water electrolytic device, the film electrode joint is excellent in strength and the electrolytic voltage are reduced, ensuring the stability of the film electrode joint under high pressure and low voltage operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004994220980000121
    Figure BDA0004994220980000121
  • Figure BDA0004994220980000131
    Figure BDA0004994220980000131
  • Figure BDA0004994220980000141
    Figure BDA0004994220980000141
Patent Text Reader

Abstract

Provided are: a membrane electrode assembly which has excellent strength and is capable of reducing electrolysis voltage when applied to a water electrolysis device; and a water electrolysis device. The membrane electrode assembly according to the present invention comprises an anode having a catalyst layer, a cathode having a catalyst layer, and a solid polymer electrolyte membrane disposed between the anode and the cathode, the membrane electrode assembly being used in a water electrolysis device, the solid polymer electrolyte membrane comprising a woven fabric and a fluorine-containing polymer having an ion exchange group, the opening ratio of the woven fabric is 50% or more, the denier number of the warp yarns and the denier number of the weft yarns constituting the woven fabric are each independently 2 or more, and the relationship Y < = 240X-170 is satisfied when the membrane thickness of the solid polymer electrolyte membrane is Y [mu] m and the ion exchange capacity of the fluorine-containing polymer is X milliequivalent per gram of dry resin.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with a filing date of February 5, 2020, an application number of 202080012825.9, and an invention name of “Membrane electrode assembly, water electrolysis device”. Technical Field

[0002] The present invention relates to a membrane electrode assembly and a water electrolysis device. Background Art

[0003] Membrane electrode assemblies including solid polymer electrolyte membranes are used in various applications and various studies have been conducted. For example, membrane electrode assemblies are used in solid polymer water electrolysis devices (Patent Document 1) and solid polymer fuel cells (Patent Document 2).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 11-021687

[0007] Patent Document 2: Japanese Patent Application Publication No. 2005-78895 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] The membrane electrode assembly used in the water electrolysis device described in Patent Document 1 may exert a greater pressure on the membrane electrode assembly divided into the anode chamber and the cathode chamber than the membrane electrode assembly used in the solid polymer fuel cell described in Patent Document 2. Therefore, the membrane electrode assembly is required to have excellent strength.

[0010] In order to reduce power consumption and obtain the target product at a lower cost, the solid polymer electrolyte membrane itself is required to have low resistance. The low resistance of the solid polymer electrolyte membrane itself means that the electrolysis voltage becomes small.

[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a membrane electrode assembly and a water electrolysis device which are excellent in strength and can reduce the electrolysis voltage when used in a water electrolysis device.

[0012] Solutions for solving problems

[0013] The inventors of the present invention have conducted in-depth research on the above-mentioned issues and found that, for a membrane electrode assembly including a solid polymer electrolyte membrane, if the solid polymer electrolyte membrane includes a fluorine-containing polymer and a woven fabric with a specified opening ratio composed of yarn of a specified denier, and the ion exchange capacity of the fluorine-containing polymer and the membrane thickness of the solid polymer electrolyte membrane satisfy a specified relationship, the desired effect can be obtained, thereby completing the present invention.

[0014] That is, the present inventors have found that the above-mentioned problems can be solved by the following configuration.

[0015] [1] A membrane electrode assembly comprising: an anode having a catalyst layer, a cathode having a catalyst layer, and a solid polymer electrolyte membrane disposed between the anode and the cathode, wherein the membrane electrode assembly is used in a water electrolysis device.

[0016] The solid polymer electrolyte membrane comprises a woven fabric and a fluorine-containing polymer having an ion exchange group.

[0017] The opening ratio of the aforementioned woven fabric is 50% or more,

[0018] The denier of the warp yarn and the denier of the weft yarn constituting the woven fabric are each independently 2 or more,

[0019] When the thickness of the solid polymer electrolyte membrane is Y μm and the ion exchange capacity of the fluorinated polymer is X milliequivalents / g of dry resin, the relationship Y≤240X-170 is satisfied.

[0020] [2] The membrane electrode assembly according to [1], wherein the opening ratio of the woven fabric is 60% or more and 80% or less.

[0021] [3] The membrane electrode assembly according to [1] or [2], wherein the denier of the warp yarn and the denier of the weft yarn constituting the woven fabric are each independently 15 or more and 50 or less.

[0022] [4] The membrane electrode assembly according to any one of [1] to [3], wherein a thickness Y of the solid polymer electrolyte membrane is 20 μm or more and 150 μm or less.

[0023] [5] The membrane electrode assembly according to any one of [1] to [4], wherein the ion exchange capacity X of the fluorinated polymer is 0.9 to 2.5 milliequivalents / g of dry resin.

[0024] [6] A membrane electrode assembly according to any one of [1] to [5], wherein the warp yarns and weft yarns constituting the woven fabric are made of a material selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, polyetheretherketone and polyphenylene sulfide.

[0025] [7] The membrane electrode assembly according to any one of [1] to [6], wherein the density of the warp yarns and the weft yarns constituting the woven fabric is 70 yarns / inch or more and 150 yarns / inch or less.

[0026] [8] The membrane electrode assembly according to any one of [1] to [7], wherein the ion exchange group is a sulfonic acid type functional group.

[0027] [9] The membrane electrode assembly according to any one of [1] to [8], wherein the fluorinated polymer comprises a unit based on a fluorinated olefin and a unit having a sulfonic acid type functional group and a fluorine atom.

[0028]

[10] The membrane electrode assembly according to [9], wherein the fluorine-containing olefin is a fluorine olefin having one or more fluorine atoms in a molecule and having 2 to 3 carbon atoms.

[0029]

[11] The membrane electrode assembly according to [9], wherein the unit having a sulfonic acid type functional group and a fluorine atom is a unit represented by formula (1).

[0030] Formula (1) - [CF 2 -CF(-L-(SO 3 M) n )]-

[0031] L is an n+1-valent perfluorocarbon group which may contain an ethereal oxygen atom, M is a hydrogen atom, an alkali metal or a quaternary ammonium cation, and n is 1 or 2.

[0032]

[12] A water electrolysis device comprising the membrane electrode assembly according to any one of [1] to

[11] .

[0033]

[13] A solid polymer electrolyte membrane, wherein the solid polymer electrolyte membrane comprises a woven fabric and a fluorine-containing polymer having an ion exchange group,

[0034] The opening ratio of the aforementioned woven fabric is 50% or more,

[0035] The denier of the warp yarn and the denier of the weft yarn constituting the woven fabric are each independently 2 or more,

[0036] When the thickness of the solid polymer electrolyte membrane is Y μm and the ion exchange capacity of the fluorinated polymer is X milliequivalents / g of dry resin, the relationship Y≤240X-170 is satisfied.

[0037] Effects of the Invention

[0038] According to the present invention, it is possible to provide a membrane electrode assembly and a water electrolysis device which are excellent in strength and can reduce the electrolysis voltage when used in a water electrolysis device. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a cross-sectional view showing an example of the membrane electrode assembly of the present invention.

[0040] Figure 2 This is a cross-sectional view showing an example of a solid polymer electrolyte membrane included in the membrane electrode assembly of the present invention.

[0041] Figure 3 It is a schematic plan view showing an example of a woven fabric included in the solid polymer electrolyte membrane of the present invention when viewed in the film thickness direction of the solid polymer electrolyte membrane.

[0042] Figure 4 This is a partial cross-sectional view for explaining the film thickness measurement position of the solid polymer electrolyte membrane of the present invention.

[0043] Figure 5 This is a graph showing the relationship between the film thickness Y of the solid polymer electrolyte and the ion exchange capacity X of the fluorinated polymer in each membrane electrode assembly produced in Examples and Comparative Examples.

[0044] Description of Reference Numerals

[0045] 10Solid polymer electrolyte membrane

[0046] 12. Electrolytes

[0047] 14. Weaving

[0048] 14a, 14b, 14c yarn

[0049] 20 membrane electrode assembly

[0050] 22 Anode

[0051] 24 cathode

[0052] 26 Catalyst layer

[0053] 28 Gas Diffusion Layer

[0054] t1, t2, t3, t4, t5, t6, t7, t8, t9 film thickness DETAILED DESCRIPTION

[0055] The definitions of the following terms apply throughout the specification and claims unless otherwise specified.

[0056] The "ion exchange group" refers to a group that can convert at least a part of ions contained in the group into other ions, and examples thereof include the following sulfonic acid type functional group and carboxylic acid type functional group.

[0057] "Sulfonic acid functional group" refers to a sulfonic acid group (-SO 3 H) or sulfonate group (-SO 3 M 2 Among them, M 2 is an alkali metal or a quaternary ammonium cation. ).

[0058] "Carboxylic acid-type functional group" refers to a carboxylic acid group (-COOH) or a carboxylate salt (-COOM 1 Among them, M 1 is an alkali metal or a quaternary ammonium cation. ).

[0059] "Precursor membrane" refers to a membrane comprising a polymer having groups that can be converted into ion exchange groups.

[0060] The "group that can be converted into an ion exchange group" refers to a group that can be converted into an ion exchange group by a treatment such as a hydrolysis treatment or an acidification treatment.

[0061] The "group that can be converted into a sulfonic acid type functional group" means a group that can be converted into a sulfonic acid type functional group by a treatment such as a hydrolysis treatment or an acidification treatment.

[0062] The "group that can be converted into a carboxylic acid type functional group" refers to a group that can be converted into a carboxylic acid type functional group by a known treatment such as a hydrolysis treatment or an acidification treatment.

[0063] The "unit" in a polymer refers to an atomic group derived from one molecule of a monomer formed by polymerization of the monomer. The unit may be an atomic group directly formed by a polymerization reaction, or an atomic group in which a part of the atomic group is converted into an atomic group of another structure by treating the polymer obtained by the polymerization reaction.

[0064] A numerical range expressed using “to” means a range including the numerical values ​​described before and after “to” as the lower limit and the upper limit.

[0065] [Membrane Electrode Assembly]

[0066] The membrane electrode assembly of the present invention comprises: an anode having a catalyst layer, a cathode having a catalyst layer, and a solid polymer electrolyte membrane arranged between the above-mentioned anode and the above-mentioned cathode. The membrane electrode assembly is used for a water electrolysis device. The above-mentioned solid polymer electrolyte membrane comprises a woven fabric and a fluorine-containing polymer having an ion exchange group (hereinafter also referred to as "fluorine-containing polymer (I)"), the opening ratio of the above-mentioned woven fabric is greater than 50%, the denier of the warp yarn and the denier of the weft yarn constituting the above-mentioned woven fabric are each independently greater than 2, and when the membrane thickness of the above-mentioned solid polymer electrolyte membrane is set to Yμm and the ion exchange capacity of the above-mentioned fluorine-containing polymer is set to X milliequivalent / gram of dry resin, the relationship of Y≤240X-170 (hereinafter also referred to as relationship Y1) is satisfied.

[0067] The membrane electrode assembly of the present invention can achieve both excellent strength and a reduction in electrolysis voltage when used in a water electrolysis device. The detailed reason for this is not clear, but it is presumed to be due to the following reasons.

[0068] As a method for improving the membrane strength of the membrane electrode assembly, a method of using a solid polymer electrolyte membrane containing a woven fabric can be cited. In particular, when a woven fabric composed of yarn with a specified denier number is used, it is preferred from the viewpoint of being able to improve the membrane strength. However, when there is a woven fabric in the solid polymer electrolyte membrane, the membrane resistance of the solid polymer electrolyte membrane is sometimes increased and the electrolysis voltage becomes higher. In response to this problem, the present inventors found that the electrolysis voltage can be reduced by using a woven fabric with a specified aperture ratio.

[0069] Furthermore, the present inventors have repeatedly studied and found that if the ion exchange capacity of the fluorinated polymer and the thickness of the solid polymer electrolyte membrane satisfy a predetermined relationship, both the improvement of the membrane strength and the reduction of the electrolysis voltage can be achieved at a higher level.

[0070] That is, the present inventors have recognized that if the ion exchange capacity of the fluorinated polymer increases, there is a tendency that the electrolysis voltage decreases, but the strength of the solid polymer electrolyte membrane decreases. In addition, it is recognized that if the thickness of the solid polymer electrolyte membrane is increased, there is a tendency that the strength of the solid polymer electrolyte membrane increases, but the electrolysis voltage increases. Based on this view, the present inventors have focused on the ion exchange capacity of the fluorinated polymer and the thickness of the solid polymer electrolyte membrane, and in order to simultaneously achieve excellent membrane strength and a reduction in electrolysis voltage, the above-mentioned relationship Y1 is derived based on the experimental results of the embodiments and comparative examples shown in the embodiment column described later.

[0071] As described above, by using a woven fabric having predetermined physical properties and a membrane electrode assembly satisfying the above-mentioned relational expression Y1, it is possible to achieve both excellent strength and a reduction in electrolysis voltage when used in a water electrolysis device.

[0072] In addition, the solid polymer electrolyte membrane included in the membrane electrode assembly of the present invention has a woven fabric with a predetermined opening ratio composed of yarns of a predetermined denier. Therefore, when the solid polymer electrolyte membrane is applied to a water electrolysis device and is transferred from a dry state to a wet state, the dimensional stability of the solid polymer electrolyte membrane is also excellent.

[0073] Figure 1 The membrane electrode assembly 20 includes an anode 22 having a catalyst layer 26 and a gas diffusion layer 28, a cathode 24 having a catalyst layer 26 and a gas diffusion layer 28, and a solid polymer electrolyte membrane 10 disposed between the anode 22 and the cathode 24 in contact with the catalyst layer 26.

[0074] <Solid Polymer Electrolyte Membrane>

[0075] Figure 2This is a cross-sectional view showing an example of a solid polymer electrolyte membrane included in the membrane electrode assembly of the present invention.

[0076] The solid polymer electrolyte membrane 10 includes an electrolyte 12 containing a fluorinated polymer (I) and a woven fabric 14 disposed in the electrolyte 12. The woven fabric 14 is composed of a yarn 14a, a yarn 14b, and a yarn 14c.

[0077] The thickness Y [μm] of the solid polymer electrolyte membrane and the ion exchange capacity X [milliequivalent / g dry resin] of the fluorinated polymer (I) satisfy the relationship Y1 (Y≤240X-170).

[0078] As described above, the relational expression Y1 is obtained from the experimental results of the examples and comparative examples shown in the example column described later. A membrane electrode assembly satisfying the relational expression Y1 has excellent strength and can reduce the electrolysis voltage when used in a water electrolysis device.

[0079] The thickness Y of the solid polymer electrolyte membrane may be appropriately set so as to satisfy the above-mentioned relational expression Y1, and is preferably 20 μm or more, more preferably 40 μm or more, and particularly preferably 70 μm or more from the viewpoint of further improving the strength of the membrane electrode assembly.

[0080] From the viewpoint of being able to further reduce the electrolysis voltage when applied to a water electrolysis device, the upper limit of the film thickness Y of the solid polymer electrolyte membrane is preferably 150 μm or less, particularly preferably 130 μm or less.

[0081] The method for calculating the film thickness Y of the solid polymer electrolyte membrane in the present invention is described below.

[0082] First, after the solid polymer electrolyte membrane is dried at 90° C. for 2 hours, the solid polymer electrolyte membrane is cut along a direction parallel to the membrane thickness direction of the solid polymer electrolyte membrane, and an enlarged image (e.g., 100 times) of the cross section of the solid polymer electrolyte membrane is taken using an optical microscope (product name "BX-51", manufactured by Olympus Corporation). It should be noted that when the solid polymer electrolyte membrane is cut, it is cut along a direction parallel to the extension direction of any one of the warp yarns and weft yarns constituting the woven fabric in the solid polymer electrolyte membrane and between the selected yarns.

[0083] use Figure 3 , the cutting position of the solid polymer electrolyte membrane is explained in more detail. Figure 3 1 is a schematic plan view of the woven fabric 14 in the solid polymer electrolyte membrane 10 when viewed in the membrane thickness direction. Figure 3 As shown, the woven fabric 14 includes: a yarn 14a, a yarn 14b, and a yarn 14c as warp yarns; and a yarn 14A, a yarn 14B, and a yarn 14C as weft yarns orthogonal to the warp yarns. Figure 3 In the example, the solid high-density electrolyte membrane 10 is cut along the weft direction and at the A-A' line located between the yarn 14A and the yarn 14B selected from the weft. Thus, Figure 2 A cross section of the solid polymer electrolyte membrane 10 as shown is exposed.

[0084] Next, using the enlarged image, select any two adjacent yarns in the cross section. And, from the center of one of the two selected yarns toward the other center, measure the thickness of the solid polymer electrolyte membrane at each point where the distance between them is advanced by 1 / 10 each time (it should be noted that the last point is the center of the other yarn, and the thickness of the membrane at this point is not measured). The membrane thickness at each point obtained in this way is taken as the arithmetic average. Among them, when the membrane thickness includes the thickness of the yarn, the membrane thickness measured at this point is not included in the calculation.

[0085] use Figure 4 The measurement position of the film thickness of the solid polymer electrolyte membrane will be described more specifically using an example. Figure 4 FIG. 1 is a partial cross-sectional view for explaining the film thickness measurement position of the solid polymer electrolyte membrane 10. Figure 4 In the example, select Figure 2 The adjacent yarns 14a and 14b are among the yarns in the embodiment. Figure 4 As shown, from point c0 as the center of yarn 14a toward point c10 as the center of yarn 14b, the film thickness t1 to film thickness t9 at points c1 to c10 except for the last point c10 are measured each time the distance therebetween advances by 1 / 10. The arithmetic mean of the thicknesses of the seven points, excluding the film thickness t1 including the thickness of yarn 14a and the film thickness t9 of yarn 14b, is calculated.

[0086] This calculation of the film thickness is performed at 10 different cross sections of the solid polymer electrolyte membrane, and the arithmetic mean of the film thicknesses at the 10 locations is taken as the film thickness Y.

[0087] (Weaving)

[0088] The opening ratio of the woven fabric is 50% or more, preferably 55% or more, and particularly preferably 60% or more, from the viewpoint of further lowering the electrolysis voltage of the water electrolysis device.

[0089] From the viewpoint of achieving better strength of the membrane electrode assembly, the upper limit of the opening ratio of the woven fabric is preferably 90% or less, particularly preferably 80% or less.

[0090] The open area ratio of the woven fabric is calculated by the following formula (ε) based on the average diameter R1 of the yarns and the average interval P1 between adjacent yarns (hereinafter also referred to as “pitch P1”).

[0091] Here, the average diameter R1 of the yarn refers to the arithmetic mean of the diameters of 10 different yarns selected at random based on the magnified image (e.g., 100 times) of the woven surface obtained using a microscope. In addition, the spacing P1 refers to the arithmetic mean of 10 points at intervals of 10 points selected at random based on the magnified image (e.g., 100 times) of the woven surface obtained using a microscope.

[0092] Opening ratio of fabric (%) = [P1 / (P1+R1)] 2 ×100(ε)

[0093] The denier of the warp yarn and the denier of the weft yarn constituting the woven fabric are each independently 2 or more, preferably 10 or more, and particularly preferably 15 or more, from the viewpoint of achieving better strength and dimensional stability of the membrane electrode assembly.

[0094] From the viewpoint of being able to further reduce the electrolysis voltage of the water electrolysis device, the upper limits of the denier of the warp yarn and the denier of the weft yarn constituting the woven fabric are each independently preferably 60 or less, particularly preferably 50 or less.

[0095] In addition, the denier is a value obtained by expressing the mass of 9000 m of yarn in grams (g / 9000 m).

[0096] Regarding the density of warp yarns and weft yarns, from the viewpoint of excellent strength and dimensional stability of the membrane electrode assembly, it is preferably 50 yarns / inch or more, and particularly preferably 70 yarns / inch or more. From the viewpoint of being able to further reduce the electrolysis voltage of the water electrolysis device, it is preferably 200 yarns / inch or less, and particularly preferably 150 yarns / inch or less.

[0097] The warp yarn and the weft yarn may be composed of either a monofilament composed of one filament or a multifilament composed of two or more filaments, and are preferably composed of a monofilament.

[0098] From the viewpoint of better durability of the yarn, the warp yarn and the weft yarn are preferably made of a material selected from the group consisting of polytetrafluoroethylene (hereinafter also referred to as "PTFE"), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (hereinafter also referred to as "PFA"), polyetheretherketone (hereinafter also referred to as "PEEK") and polyphenylene sulfide (hereinafter also referred to as "PPS").

[0099] From the viewpoint of achieving better durability and strength of the yarn, the warp yarn and the weft yarn are preferably composed of slit yarn.

[0100] In woven fabrics, the warp yarns and the weft yarns are preferably orthogonal.

[0101] When the material constituting the woven fabric is PTFE, the weight per unit area of ​​the woven fabric is preferably 20 to 40 g / m2 from the viewpoint of excellent balance between the strength and handling properties of the solid polymer electrolyte membrane. 2 , particularly preferably 30 to 40 g / m 2 .

[0102] When the material constituting the woven fabric is PFA, the weight per unit area of ​​the woven fabric is preferably 10 to 30 g / m2 from the viewpoint of excellent balance between the strength and handling properties of the solid polymer electrolyte membrane. 2 , particularly preferably 10 to 20 g / m 2 .

[0103] When the material constituting the woven fabric is PEEK, the weight per unit area of ​​the woven fabric is preferably 5 to 40 g / m2 from the viewpoint of excellent balance between the strength and handling properties of the solid polymer electrolyte membrane. 2 , particularly preferably 5 to 30 g / m 2 .

[0104] When the material constituting the woven fabric is PPS, the weight per unit area of ​​the woven fabric is preferably 5 to 40 g / m2 from the viewpoint of excellent balance between the strength and handling properties of the solid polymer electrolyte membrane. 2 , particularly preferably 5 to 30 g / m 2 .

[0105] (Electrolytes)

[0106] The electrolyte contains a fluorine-containing polymer (I).

[0107] From the viewpoint of satisfying both excellent membrane strength and reduction in electrolysis voltage at a higher level, the ion exchange capacity X of the fluoropolymer (I) is preferably 0.9 to 2.5 milliequivalents / g of dry resin, more preferably 1.0 to 2.3 milliequivalents / g of dry resin, particularly preferably 1.0 to 2.0 milliequivalents / g of dry resin.

[0108] The fluorinated polymer (I) used in the solid polymer electrolyte membrane may be one kind or two or more kinds may be laminated or mixed and used.

[0109] The solid polymer electrolyte membrane may contain a polymer other than the fluorinated polymer (I), and the polymer in the solid polymer electrolyte membrane is preferably substantially composed of the fluorinated polymer (I). Substantially composed of the fluorinated polymer (I) means that the content of the fluorinated polymer (I) is 95% by mass or more relative to the total mass of the polymer in the solid polymer electrolyte membrane. As the upper limit of the content of the fluorinated polymer (I), it can be listed that the total mass of the polymer in the solid polymer electrolyte membrane is 100% by mass.

[0110] Specific examples of the other polymers other than the fluorinated polymer (I) include one or more polyazole compounds selected from the group consisting of polymers of heterocyclic compounds containing one or more nitrogen atoms in the ring and polymers of heterocyclic compounds containing one or more nitrogen atoms in the ring and containing oxygen atoms and / or sulfur atoms.

[0111] Specific examples of the polyazole compound include polyimidazole compounds, polybenzimidazole compounds, polybenzbisimidazole compounds, polybenzoxazole compounds, polyoxazole compounds, polythiazole compounds, and polybenzothiazole compounds.

[0112] In addition, from the viewpoint of oxidation resistance of the solid polymer electrolyte membrane, other polymers include polyphenylene sulfide resin and polyphenylene ether resin.

[0113] The fluorinated polymer (I) has an ion exchange group. Specific examples of the ion exchange group include a sulfonic acid type functional group and a carboxylic acid type functional group. From the viewpoint of being able to further reduce the electrolysis voltage, a sulfonic acid type functional group is preferred.

[0114] Hereinafter, an embodiment of the fluorinated polymer having a sulfonic acid type functional group (hereinafter also referred to as “fluorinated polymer (S)”) will be described in detail.

[0115] The fluorine-containing polymer (S) preferably contains a fluorine-containing olefin-based unit and a unit having a sulfonic acid type functional group and a fluorine atom.

[0116] Examples of the fluorinated olefin include fluorinated olefins having one or more fluorine atoms in the molecule and having 2 to 3 carbon atoms. Specific examples of the fluorinated olefin include tetrafluoroethylene (hereinafter also referred to as "TFE"), chlorotrifluoroethylene, vinylidene fluoride, vinyl fluoride, and hexafluoropropylene. Among them, TFE is preferred from the viewpoint of the production cost of the monomer, the reactivity with other monomers, and the excellent properties of the obtained fluorinated polymer (S).

[0117] The fluorinated olefins may be used alone or in combination of two or more.

[0118] As the unit having a sulfonic acid type functional group and a fluorine atom, a unit represented by formula (1) is preferred.

[0119] Formula (1) - [CF 2 -CF(-L-(SO 3 M) n )]-

[0120] L is an n+1-valent perfluorocarbon group which may contain an etheric oxygen atom.

[0121] The etheric oxygen atom may be located at the terminal of the perfluorocarbon group or between carbon atoms.

[0122] The number of carbon atoms in the n+1-valent perfluorocarbon group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.

[0123] L is preferably an n+1-valent perfluoroaliphatic hydrocarbon group optionally containing an etheric oxygen atom, and particularly preferably a divalent perfluoroalkylene group optionally containing an etheric oxygen atom in which n=1 is present, or a trivalent perfluoroaliphatic hydrocarbon group optionally containing an etheric oxygen atom in which n=2 is present.

[0124] The divalent perfluoroalkylene group may be either linear or branched.

[0125] M is a hydrogen atom, an alkali metal or a quaternary ammonium cation.

[0126] n is 1 or 2.

[0127] The unit represented by formula (1) is preferably a unit represented by formula (1-1), a unit represented by formula (1-2), a unit represented by formula (1-3), or a unit represented by formula (1-4).

[0128] Formula (1-1)-[CF 2 -CF(-OR f1 -SO 3 M)]-

[0129] Formula (1-2)-[CF 2 -CF(-R f1 -SO 3 M)]-

[0130]

[0131] R f1 The perfluoroalkylene group is a perfluoroalkylene group which may contain an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.

[0132] R f2 The perfluoroalkylene group is a single bond or optionally contains an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.

[0133] R f3 The perfluoroalkylene group is a single bond or optionally contains an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.

[0134] r is 0 or 1.

[0135] m is 0 or 1.

[0136] M is a hydrogen atom, an alkali metal or a quaternary ammonium cation.

[0137] As the unit represented by the formula (1-1) and the unit represented by the formula (1-2), the unit represented by the formula (1-5) is more preferable.

[0138] Formula (1-5)-[CF 2 -CF(-(CF 2 ) x -(OCF 2 CFY) y -O-(CF 2 ) z -SO 3 M)] - x is 0 or 1, y is an integer from 0 to 2, z is an integer from 1 to 4, and Y is F or CF 3 . M as described above.

[0139] Specific examples of the unit represented by formula (1-1) include the following units: w in the formula is an integer of 1 to 8, and x is an integer of 1 to 5. M in the formula has the same meaning as described above.

[0140] -[CF 2 -CF(-O-(CF 2 ) w -SO 3 M)]-

[0141] -[CF 2 -CF(-O-CF 2 CF(CF 3 )-O-(CF 2 ) w -SO 3 M)]-

[0142] -[CF 2 -CF(-(O-CF 2 CF(CF 3 )) x -SO 3 M)]-

[0143] Specific examples of the unit represented by formula (1-2) include the following units: w in the formula is an integer of 1 to 8. M in the formula has the same meaning as described above.

[0144] -[CF 2 -CF(-(CF 2 ) w -SO 3 M)]-

[0145] -[CF 2 -CF(-CF 2 -O-(CF 2 ) w -SO 3 M)]-

[0146] The unit represented by the formula (1-3) is preferably a unit represented by the formula (1-3-1). M in the formula has the same meaning as described above.

[0147]

[0148] R f4 is a linear perfluoroalkylene group having 1 to 6 carbon atoms, R f5 It is a single bond or a linear perfluoroalkylene group having 1 to 6 carbon atoms which may contain an oxygen atom between carbon atoms. r and M are as defined above.

[0149] Specific examples of the unit represented by formula (1-3-1) include the following.

[0150]

[0151] The unit represented by formula (1-4) is preferably a unit represented by formula (1-4-1). f1 , R f2 and M are defined as above.

[0152]

[0153] Specific examples of the unit represented by formula (1-4-1) include the following.

[0154]

[0155] The unit having a sulfonic acid type functional group and a fluorine atom may be used alone or in combination of two or more.

[0156] The fluorine-containing polymer (I) optionally contains units based on other monomers in addition to the units based on the fluorine-containing olefin and the units having a sulfonic acid type functional group and a fluorine atom.

[0157] Specific examples of other monomers include CF 2 =CFR f6 (Among them, R f6 is a perfluoroalkyl group having 2 to 10 carbon atoms), CF 2 =CF-OR f7 (Among them, R f7 is a perfluoroalkyl group having 1 to 10 carbon atoms), CF 2 =CFO(CF2 ) v CF=CF 2 (wherein v is an integer from 1 to 3).

[0158] From the viewpoint of maintaining the ion exchange performance, the content of the units derived from other monomers is preferably at most 30 mass % based on all the units in the fluorinated polymer (I).

[0159] The solid polymer electrolyte membrane may have a single-layer structure or a multi-layer structure. In the case of a multi-layer structure, for example, a plurality of layers containing the fluorinated polymer (I) and having different ion exchange capacities may be stacked.

[0160] (Method for producing solid polymer electrolyte membrane)

[0161] The solid polymer electrolyte membrane is preferably manufactured as follows: a membrane (hereinafter also referred to as a "precursor membrane") is manufactured comprising a woven fabric and a polymer (hereinafter also referred to as a "fluorinated polymer (I')") having a fluorinated monomer (hereinafter also referred to as a fluorinated monomer (I')) having a group that can be converted into an ion exchange group, and then the groups in the precursor membrane that can be converted into an ion exchange group are converted into ion exchange groups.

[0162] The form of the woven fabric is as described above.

[0163] As the fluorinated polymer (I'), a polymer (hereinafter also referred to as "fluorinated monomer (S')") having a group that can be converted into a sulfonic acid type functional group is preferred, and a copolymer of a fluorinated olefin and a monomer having a group that can be converted into a sulfonic acid type functional group and a fluorine atom is particularly preferred.

[0164] The fluorinated polymer (S') will be described in detail below.

[0165] As the copolymerization method of the fluorinated polymer (S'), known methods such as solution polymerization, suspension polymerization and emulsion polymerization can be adopted.

[0166] Examples of the fluorinated olefin include the fluorinated olefins exemplified above, and TFE is preferred from the viewpoint of the production cost of the monomer, the reactivity with other monomers, and the excellent properties of the fluorinated polymer (S) to be obtained.

[0167] The fluorinated olefins may be used alone or in combination of two or more.

[0168] Examples of the fluorine-containing monomer (S′) include compounds having one or more fluorine atoms in the molecule, having an ethylenic double bond, and having a group that can be converted into a sulfonic acid type functional group.

[0169] The fluorinated monomer (S') is preferably a compound represented by the formula (2) from the viewpoint of the production cost of the monomer, the reactivity with other monomers, and the excellent properties of the obtainable fluorinated polymer (S).

[0170] Formula (2) CF 2 =CF-L-(A) n

[0171] L and n in formula (2) are as defined above.

[0172] A is a group that can be converted into a sulfonic acid type functional group. The group that can be converted into a sulfonic acid type functional group is preferably a functional group that can be converted into a sulfonic acid type functional group by hydrolysis. Specific examples of the group that can be converted into a sulfonic acid type functional group include -SO 2 F, -SO 2 Cl, -SO 2 Br.

[0173] The compound represented by formula (2) is preferably a compound represented by formula (2-1), a compound represented by formula (2-2), a compound represented by formula (2-3), and a compound represented by formula (2-4).

[0174] Formula (2-1) CF 2 =CF-OR f1 -A

[0175] Formula (2-2) CF 2 =CF-R f1 -A

[0176]

[0177] R in the formula f1 , R f2 , r and A are defined as above.

[0178]

[0179] R in the formula f1 , R f2 , R f3 , r, m and A are defined as above.

[0180] As the compound represented by the formula (2-1) and the compound represented by the formula (2-1), the compound represented by the formula (2-5) is preferred.

[0181] Formula (2-5) CF 2 =CF-(CF 2 ) x -(OCF 2 CFY) y -O-(CF2 ) z -SO 3 M

[0182] In the formula, M, x, y, z and Y are as defined above.

[0183] Specific examples of the compound represented by formula (2-1) include the following compounds: wherein w is an integer of 1 to 8, and x is an integer of 1 to 5.

[0184] CF 2 =CF-O-(CF 2 ) w -SO 2 F

[0185] CF 2 =CF-O-CF 2 CF(CF 3 )-O-(CF 2 ) w -SO 2 F

[0186] CF 2 =CF-[O-CF 2 CF(CF 3 )] x -SO 2 F

[0187] Specific examples of the compound represented by formula (2-2) include the following compounds: wherein w in the formula is an integer of 1 to 8.

[0188] CF 2 =CF-(CF 2 ) w -SO 2 F

[0189] CF 2 =CF-CF 2 -O-(CF 2 ) w -SO 2 F

[0190] The compound represented by the formula (2-3) is preferably a compound represented by the formula (2-3-1).

[0191]

[0192] R in the formula f4 , R f5 , r and A are defined as above.

[0193] Specific examples of the compound represented by formula (2-3-1) include the following.

[0194]

[0195] The compound represented by the formula (2-4) is preferably a compound represented by the formula (2-4-1).

[0196]

[0197] R in the formula f1 , R f2 and A are defined as above.

[0198] Specific examples of the compound represented by formula (2-4-1) include the following.

[0199]

[0200] The fluorinated monomer (S') may be used alone or in combination of two or more.

[0201] In the production of the fluorinated polymer (S'), other monomers may be used in addition to the fluorinated olefin and the fluorinated monomer (S'). Examples of the other monomers include the monomers exemplified above.

[0202] The ion exchange capacity of the fluorinated polymer (I') can be adjusted by changing the content of the group convertible into an ion exchange group in the fluorinated polymer (I').

[0203] As a specific example of the method for producing the precursor film, an extrusion method can be cited. More specifically, the following method can be cited: forming a film (I') containing a fluorinated polymer (I'), then arranging the film (I'), the woven fabric, and the film (I') in this order, and laminating them using a laminating roll or a vacuum laminating device.

[0204] Specific examples of the method for converting the groups in the precursor film that can be converted into ion exchange groups into ion exchange groups include a method of subjecting the precursor film to a treatment such as a hydrolysis treatment or an acidification treatment.

[0205] Among them, a method of bringing the precursor film into contact with an alkaline aqueous solution is preferred.

[0206] Specific examples of the method of bringing the precursor film into contact with the alkaline aqueous solution include a method of immersing the precursor film in the alkaline aqueous solution and a method of spraying the alkaline aqueous solution on the surface of the precursor film.

[0207] The temperature of the alkaline aqueous solution is preferably 30 to 100° C., particularly preferably 40 to 100° C. The contact time between the precursor film and the alkaline aqueous solution is preferably 3 to 150 minutes, particularly preferably 5 to 50 minutes.

[0208] The alkaline aqueous solution preferably contains an alkali metal hydroxide, a water-soluble organic solvent and water.

[0209] Examples of the alkali metal hydroxide include sodium hydroxide and potassium hydroxide.

[0210] In this specification, the water-soluble organic solvent refers to an organic solvent that is easily soluble in water, and specifically, an organic solvent having a solubility of 0.1 g or more in 1000 ml (20° C.) of water is preferred, and an organic solvent having a solubility of 0.5 g or more is particularly preferred. The water-soluble organic solvent preferably includes at least one selected from the group consisting of aprotic organic solvents, alcohols, and amino alcohols, and particularly preferably includes an aprotic organic solvent.

[0211] The water-soluble organic solvent may be used alone or in combination of two or more.

[0212] Specific examples of the aprotic organic solvent include dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone, and dimethyl sulfoxide is preferred.

[0213] Specific examples of the alcohols include methanol, ethanol, isopropanol, butanol, methoxyethoxyethanol, butoxyethanol, butyl carbitol, hexyloxyethanol, octanol, 1-methoxy-2-propanol, and ethylene glycol.

[0214] Specific examples of amino alcohols include ethanolamine, N-methylethanolamine, N-ethylethanolamine, 1-amino-2-propanol, 1-amino-3-propanol, 2-aminoethoxyethanol, 2-aminothioethoxyethanol, and 2-amino-2-methyl-1-propanol.

[0215] The concentration of the alkali metal hydroxide in the alkaline aqueous solution is preferably 1 to 60% by mass, particularly preferably 3 to 55% by mass.

[0216] The content of the water-soluble organic solvent in the alkaline aqueous solution is preferably 1 to 60% by mass, particularly preferably 3 to 55% by mass.

[0217] The concentration of water in the alkaline aqueous solution is preferably 39 to 80% by mass.

[0218] After the precursor film is brought into contact with the alkaline aqueous solution, a treatment to remove the alkaline aqueous solution may be performed. Examples of the method for removing the alkaline aqueous solution include a method of washing the precursor film brought into contact with the alkaline aqueous solution with water.

[0219] After the precursor film is contacted with the alkaline aqueous solution, the resulting film can be contacted with an acidic aqueous solution to convert the ion exchange groups to the acid form.

[0220] Specific examples of the method of bringing the precursor film into contact with the acidic aqueous solution include a method of immersing the precursor film in the acidic aqueous solution and a method of spraying the acidic aqueous solution on the surface of the precursor film.

[0221] The acidic aqueous solution preferably contains an acid component and water.

[0222] Specific examples of the acid component include hydrochloric acid and sulfuric acid.

[0223] <Anode and cathode>

[0224] The anode and the cathode each have a catalyst layer. Figure 2 In the example shown in FIG. 1 , the anode 22 and the cathode 24 have a catalyst layer 26 and a gas diffusion layer 28 , respectively.

[0225] Specific examples of the catalyst layer include a layer containing a catalyst and a polymer having an ion exchange group.

[0226] Specific examples of the catalyst include: a supported catalyst in which a catalyst containing platinum, a platinum alloy, or platinum having a core-shell structure is supported on a carbon support; an iridium oxide catalyst; an alloy containing iridium oxide, or a catalyst containing iridium oxide having a core-shell structure. As the carbon support, carbon black powder may be cited.

[0227] Examples of the polymer having an ion exchange group include fluorine-containing polymers having an ion exchange group.

[0228] The gas diffusion layer has a function of uniformly diffusing the gas in the catalyst layer and a function of serving as a current collector. Specific examples of the gas diffusion layer include carbon paper, carbon cloth, and carbon felt.

[0229] The gas diffusion layer is preferably subjected to water-repellent treatment using PTFE or the like.

[0230] Figure 1 The membrane electrode assembly includes a gas diffusion layer 28, which is an arbitrary member and may not be included in the membrane electrode assembly.

[0231] <Method for Manufacturing Membrane Electrode Assembly>

[0232] As methods for manufacturing membrane electrode assemblies, the following methods can be listed, for example: a method in which a catalyst layer is formed on a solid polymer electrolyte membrane and the resulting assembly is further clamped by a gas diffusion layer; and a method in which a catalyst layer is formed on a gas diffusion layer to form an electrode (anode, cathode), and the solid polymer electrolyte membrane is clamped by the electrode.

[0233] The catalyst layer can be produced by applying a catalyst layer-forming coating liquid to a predetermined position and drying it as needed. The catalyst layer-forming coating liquid is a liquid obtained by dispersing a polymer having an ion exchange group and a catalyst in a dispersion medium.

[0234] <Purpose>

[0235] The membrane electrode assembly of the present invention is used in a water electrolysis device (specifically, a solid polymer water electrolysis device). The membrane electrode assembly in the water electrolysis device is arranged at a position that is separated into an anode chamber and a cathode chamber. Therefore, when the water electrolysis device is operated, a large pressure is sometimes applied to the membrane electrode assembly. Even in this case, the membrane strength of the membrane electrode assembly of the present invention is excellent, so it is possible to suppress the damage of the membrane electrode assembly when it is used in the water electrolysis device.

[0236] [Water electrolysis device]

[0237] The water electrolysis device of the present invention includes the membrane electrode assembly described above. The membrane electrode assembly of the present invention is excellent in strength, and therefore the water electrolysis device of the present invention is excellent in durability. In addition, the water electrolysis device of the present invention can reduce the electrolysis voltage.

[0238] Example

[0239] Hereinafter, the present invention will be described in detail with reference to Examples, but the present invention is not limited to these Examples.

[0240] [film thickness]

[0241] The film thickness Y of the solid polymer electrolyte membrane is calculated according to the method described in the above-mentioned column of the description of the solid polymer electrolyte membrane.

[0242] [Ion exchange capacity of fluorinated polymer]

[0243] The fluoropolymer was placed in a glove box with dry nitrogen flowing for 24 hours, and the dry mass of the fluoropolymer was measured. Thereafter, the fluoropolymer was immersed in a 2 mol / L sodium chloride aqueous solution at 60°C for 1 hour. The fluoropolymer was washed with ultrapure water and then taken out, and the liquid immersed in the fluoropolymer was titrated with a 0.1 mol / L sodium hydroxide aqueous solution to obtain the ion exchange capacity X (milliequivalent / g dry resin) of the fluoropolymer.

[0244] [Weight per unit area of ​​woven fabric]

[0245] The original roll of woven fabric used was cut into a size of 20×20 cm and the mass was measured. The above measurement was performed 5 times and the weight per unit area of ​​the woven fabric (g / m 2 ).

[0246] [The density of the warp and weft yarns that make up the fabric]

[0247] The density of the warp and weft yarns constituting the woven fabric was calculated as follows: For each of the warp and weft yarns, the length of 10 yarns was measured five times based on an image observed with an optical microscope, and the average value was converted into density (threads / inch) for calculation.

[0248] [Opening ratio of fabric]

[0249] The calculation was performed by the method described in the column of the description of the above-mentioned woven fabric using a sample cut into a size of 20×20 cm from the original roll of the woven fabric used.

[0250] [Denier of warp yarn and denier of weft yarn constituting woven fabric]

[0251] The denier of the warp yarn and the denier of the weft yarn constituting the woven fabric were calculated as follows: Five opening areas were randomly selected, and the opening ratio was calculated from the image observed by an optical microscope, and the average value was taken as the opening ratio.

[0252] [Burst test]

[0253] The membrane electrode assembly obtained in the following step was subjected to five burst tests using a Mullen burst tester M2-LD (manufactured by Toyo Seiki Seisaku-sho, Ltd.), and evaluation was performed based on the average of the five measured values ​​(burst strength) according to the following criteria.

[0254] ◎:400kPa or more

[0255] 0: More than 210 kPa and less than 400 kPa

[0256] ×: Below 210kPa

[0257] [Electrolysis voltage evaluation test]

[0258] TFE and the monomer (X) described below were copolymerized, and the polymer was made into an acid form after hydrolysis and acid treatment. The obtained polymer (ion exchange capacity: 1.10 milliequivalents / g dry resin) was dispersed in a solvent of water / ethanol = 40 / 60 (mass %) at a solid content concentration of 25.8% to obtain a dispersion (hereinafter also referred to as "dispersion X"). Ethanol (0.52 g) and water (3.34 g) were added to the obtained dispersion X (19.0 g), and an iridium oxide catalyst ("ELC-1910" manufactured by Tanaka Kikinzoku Co., Ltd.) (13.0 g) containing 76% by mass of iridium was further added to the dispersion. After the obtained mixture was treated with a planetary bead mill (rotation speed of 300 rpm) for 30 minutes, water (4.49 g) and ethanol (4.53 g) were added, and further treated with a planetary bead mill (rotation speed of 200 rpm) for 60 minutes to obtain an anode catalyst ink having a solid content concentration of 40% by mass.

[0259] On one surface of the solid polymer electrolyte membrane obtained by the steps described later, iridium was coated at a concentration of 2.0 mg / cm 2 The anode catalyst ink was applied in a manner of , dried at 80° C. for 10 minutes, and further heat treated at 150° C. for 15 minutes to obtain an electrolyte membrane with an anode catalyst layer.

[0260] Water (59.4 g) and ethanol (39.6 g) were added to a supported catalyst (“TEC10E50E” manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) (11 g) obtained by supporting 46 mass % of platinum on carbon powder, and mixed and pulverized using an ultrasonic homogenizer to obtain a catalyst dispersion.

[0261] To the catalyst dispersion, a mixed solution (29.2 g) obtained by mixing and kneading the pre-mixed dispersion X (20.1 g), ethanol (11 g) and ZEOLORA-H (manufactured by ZEON Corporation, Japan) (6.3 g) was added. Furthermore, water (3.66 g) and ethanol (7.63 g) were added to the obtained dispersion, and mixed for 60 minutes using a paint mixer to adjust the solid content concentration to 10.0% by mass, thereby obtaining a cathode catalyst ink.

[0262] The cathode catalyst ink was applied to an ETFE sheet using a die coater, dried at 80°C, and further heat treated at 150°C for 15 minutes to obtain a platinum content of 0.4 mg / cm 2 Cathode catalyst layer decoration.

[0263] The surface of the electrolyte membrane with the anode catalyst layer without the anode catalyst layer is made opposite to the surface of the cathode catalyst layer decoration with the catalyst layer, and the electrolyte membrane with the anode catalyst layer and the cathode catalyst layer are heated and pressed under the conditions of a pressing temperature of 150°C, a pressing time of 2 minutes, and a pressure of 3MPa to join the electrolyte membrane with the anode catalyst layer and the cathode catalyst layer. After the temperature is lowered to 70°C, the pressure is released and the electrolyte membrane is taken out, and the ETFE sheet of the cathode catalyst layer decoration is peeled off to obtain an electrode with an area of ​​25cm 2 membrane electrode assembly.

[0264] The membrane electrode assembly obtained through the above steps was heat-treated at 150° C. for 15 minutes and then mounted on a water electrolysis evaluation jig EH50-25 (manufactured by Greenlight Innovation Co., Ltd.).

[0265] Next, first, in order to fully hydrate the solid polymer electrolyte membrane and the two electrode ionomers, pure water at 80°C and a conductivity of 1.0 μS / cm or less was supplied to the anode and cathode sides at a flow rate of 50 mL / min for 12 hours. Thereafter, the cathode side was purged with nitrogen.

[0266] After nitrogen purging, atmospheric pressure pure water with a conductivity of less than 1.0 μS / cm and a temperature of 80°C was supplied to the anode side at a flow rate of 50 mL / min, and the generated gas pressure on the cathode side was kept at atmospheric pressure while using a DC power supply PWR1600L manufactured by Kikusui Electronics Industry Co., Ltd. at a current density of 0 to 50 A (current density of 0 to 2 A / cm 2 ) range, and the current was increased by 2.5 A at a time. The current was maintained for 10 minutes at each stage, and the current was evaluated according to the following criteria: 50 A (current density 2 A / cm 2 ) when the electrolysis voltage is

[0267] ◎:1.85V or less

[0268] ○: greater than 1.85V and less than 1.95V

[0269] ×: greater than 1.95V

[0270] [Production of fluorinated polymer (S'-1)]

[0271] CF 2 =CF 2 The monomer (X) represented by the following formula (X) was copolymerized to obtain a fluorinated polymer (S'-1) (ion exchange capacity: 1.25 meq / g dry resin).

[0272] CF 2 =CF-O-CF 2 CF(CF 3 )-O-CF2 CF 2 -SO 2 F···(X)

[0273] [Production of fluorinated polymer (S'-2)]

[0274] CF 2 =CF 2 The monomer (Y) represented by the following formula (Y) was copolymerized to obtain a fluorinated polymer (S'-2) (ion exchange capacity: 1.90 meq / g dry resin).

[0275]

[0276] [Production of fluorinated polymer (S'-3)]

[0277] CF 2 =CF 2 By copolymerizing with the monomer (X), a fluorinated polymer (S'-3) (ion exchange capacity: 1.00 meq / g dry resin) was obtained.

[0278] [Production of fluorinated polymer (S'-4)]

[0279] CF 2 =CF 2 The monomer (Z) represented by the following formula (Z) was copolymerized to obtain a fluorinated polymer (S'-4) (ion exchange capacity: 1.78 meq / g dry resin).

[0280]

[0281] The ion exchange capacities described in the above [Production of fluorinated polymer (S'-1)] to [Production of fluorinated polymer (S'-4)] represent the ion exchange capacities of fluorinated polymers obtained when fluorinated polymers (S'-1) to (S'-4) are hydrolyzed by the steps described later.

[0282] [Manufacturing of Film α1]

[0283] The fluorinated polymer (S'-1) was molded by a melt extrusion method to obtain a film α1 (film thickness: 45 μm) composed of the fluorinated polymer (S'-1).

[0284] [Manufacturing of Film α2]

[0285] The fluorinated polymer (S'-1) was molded by a melt extrusion method to obtain a film α2 (film thickness: 30 μm) composed of the fluorinated polymer (S'-1).

[0286] [Manufacturing of Film α3]

[0287] The fluorinated polymer (S'-1) was molded by a melt extrusion method to obtain a film α3 (film thickness: 60 μm) composed of the fluorinated polymer (S'-1).

[0288] [Manufacturing of Film α4]

[0289] The fluorinated polymer (S'-1) was molded by a melt extrusion method to obtain a film α4 (film thickness: 70 μm) composed of the fluorinated polymer (S'-1).

[0290] [Manufacturing of Film β1]

[0291] The fluorinated polymer (S'-2) was molded by a melt extrusion method to obtain a film β1 (film thickness: 70 μm) composed of the fluorinated polymer (S'-2).

[0292] [Manufacturing of Thin Film γ1]

[0293] The fluorinated polymer (S'-3) was molded by a melt extrusion method to obtain a thin film γ1 (film thickness: 30 μm) composed of the fluorinated polymer (S'-3).

[0294] [Manufacturing of thin film σ1]

[0295] The fluorinated polymer (S'-4) was molded by a melt extrusion method to obtain a film σ1 (film thickness: 70 μm) composed of the fluorinated polymer (S'-4).

[0296] [Manufacture of woven fabrics]

[0297] PPS yarns with a denier of 11.7 were used as warp and weft yarns, and the yarn density was 100 yarns / inch to obtain fabric A1. The weight per unit area of ​​fabric A1 was 10.2 g / m 2 It should be noted that the warp yarn and the weft yarn are composed of slit film flat yarns.

[0298] In addition, except that the type and denier of the material constituting the warp and weft yarns, and the density and unit area weight of the woven fabric were changed so as to reach the values ​​recorded in Table 1, the same operation as the production of the woven fabric A1 was carried out to produce woven fabrics A2 to A4, B1 to B2, C1 to C2 and D1.

[0299] [Example 1]

[0300] PET film / film α1 / woven fabric A1 / film α1 / PET film are stacked in this order. The stacked components are heated to 200°C and subjected to a surface pressure of 30 MPa / m 2 After heating and pressing for 10 minutes with a flat plate press, both sides of the transfer substrate were peeled off at a temperature of 50° C. to obtain a precursor film.

[0301] The precursor film was immersed in a solution of dimethyl sulfoxide / potassium hydroxide / water = 30 / 5.5 / 64.5 (mass ratio) at 95°C for 30 minutes to hydrolyze the groups in the precursor film that can be converted into sulfonic acid-type functional groups and convert them into K-type sulfonic acid-type functional groups, and then washed with water. Thereafter, the obtained film was immersed in 1M sulfuric acid to convert the terminal groups from K-type to H-type, and then dried to obtain a solid polymer electrolyte membrane.

[0302] The obtained solid polymer electrolyte membrane was used to carry out measurement of the film thickness Y of the solid polymer electrolyte membrane, a rupture test, and a water electrolysis performance evaluation test.

[0303] [Examples 2 to 11, Comparative Examples 1 to 8]

[0304] A solid polymer electrolyte membrane was prepared by the same method as in Example 1 except that the types of film and woven fabric were changed as described in Table 1, and the thickness Y of the solid polymer electrolyte membrane was measured and various tests were performed. However, no woven fabric was used in Comparative Examples 1 and 2. The results are shown in Table 1.

[0305] The "denier (g / 9000m)" in Table 1 indicates the denier of the warp and weft yarns constituting the woven fabric. In Examples 1 to 11 and Comparative Examples 1 to 8, the denier of the warp and weft yarns constituting the woven fabric was the same.

[0306] [Table 1]

[0307]

[0308] Figure 5 The graph is obtained by plotting each membrane electrode assembly of the embodiment and the comparative example, with the ion exchange capacity X of the fluorinated polymer contained in the solid polymer electrolyte membrane as the horizontal axis and the membrane thickness Y of the solid polymer electrolyte membrane as the vertical axis. It should be noted that the dotted line in the figure is the straight line represented by the formula Y=240X-170.

[0309] like Figure 5 It can be seen from the figure that the membrane electrode assemblies of Examples 1 to 11 all satisfy the relationship Y1 (ie, Y≤240X-170).

[0310] As shown in Table 1, it can be confirmed that when a membrane electrode assembly using a woven fabric having an opening ratio of 50% or more and a denier of the warp yarn and a denier of the weft yarn each independently being 2 or more, and comprising a solid polymer electrolyte membrane satisfying the relationship Y1, has excellent strength and can reduce the electrolysis voltage when used in a water electrolysis device (Examples 1 to 11).

[0311] On the other hand, although the membrane electrode assemblies of Comparative Examples 1 and 2 satisfy the formula of Y≤240X-170, since a solid polymer electrolyte membrane containing no woven fabric is used, the strength of the membrane electrode assemblies is poor.

[0312] Furthermore, although the membrane electrode assemblies of Comparative Examples 3 to 5 satisfy the formula Y≤240X-170, they use woven fabrics having an opening ratio of less than 50%, and therefore, the electrolysis voltage becomes high when used in a water electrolysis device.

[0313] In addition, the membrane electrode assemblies of Comparative Examples 6 and 7 use woven fabrics with an opening ratio of more than 50% and a denier of the warp yarn and a denier of the weft yarn that are each independently more than 2, but do not satisfy the formula Y≤240X-170. Therefore, when used in a water electrolysis device, the electrolysis voltage becomes high.

[0314] In addition, although the membrane electrode assembly of Comparative Example 8 satisfied the formula of Y≤240X-170, a woven fabric having a warp yarn denier and a weft yarn denier of less than 2 was used, and therefore the strength of the membrane electrode assembly was poor.

[0315] It should be noted that the entire contents of the specification, claims, and abstract of Japanese Patent Application No. 2019-021696 filed on February 8, 2019 are cited here and incorporated herein as the disclosed contents of the specification of the present invention.

Claims

1. A membrane electrode assembly comprising: an anode having a catalyst layer, a cathode having a catalyst layer, and a solid polymer electrolyte membrane disposed between the anode and the cathode, wherein the membrane electrode assembly is used in a water electrolysis device. The solid polymer electrolyte membrane comprises a woven fabric and a fluorine-containing polymer having an ion exchange group. The opening ratio of the woven fabric is more than 50%, The denier of the warp yarn and the denier of the weft yarn constituting the woven fabric are each independently 2 or more, When the thickness of the solid polymer electrolyte membrane is Y μm and the ion exchange capacity of the fluorinated polymer is X milliequivalents / g dry resin, the relationship Y≤240X-170 is satisfied. The density of the warp yarns and the weft yarns constituting the woven fabric is more than 150 yarns / inch and less than or equal to 200 yarns / inch.

2. The membrane electrode assembly according to claim 1, in, The opening ratio of the woven fabric is 60% or more and 80% or less.

3. The membrane electrode assembly according to claim 1 or 2, in, The denier of the warp yarn and the denier of the weft yarn constituting the woven fabric are each independently 15 or more and 50 or less.

4. The membrane electrode assembly according to claim 1 or 2, in, The solid polymer electrolyte membrane has a thickness Y of 20 μm or more and 150 μm or less.

5. The membrane electrode assembly according to claim 1 or 2, in, The ion exchange capacity X of the fluorine-containing polymer is 0.9 to 2.5 milliequivalents per gram of dry resin.

6. The membrane electrode assembly according to claim 1 or 2, in, The warp yarns and the weft yarns constituting the woven fabric are composed of a material selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, polyetheretherketone, and polyphenylene sulfide.

7. The membrane electrode assembly according to claim 1 or 2, in, The ion exchange group is a sulfonic acid type functional group.

8. The membrane electrode assembly according to claim 1 or 2, in, The fluorine-containing polymer comprises a unit based on a fluorine-containing olefin and a unit having a sulfonic acid type functional group and a fluorine atom.

9. The membrane electrode assembly according to claim 8, in, The fluorine-containing olefin is a fluorine olefin having one or more fluorine atoms in the molecule and having 2 to 3 carbon atoms.

10. The membrane electrode assembly according to claim 8, in, The unit having a sulfonic acid type functional group and a fluorine atom is a unit represented by formula (1), Formula (1)-[CF 2 -CF(-L-(SO 3 M) n )]- L is an n+1-valent perfluorocarbon group which may contain an ethereal oxygen atom, M is a hydrogen atom, an alkali metal or a quaternary ammonium cation, and n is 1 or 2. 11 . A water electrolysis device comprising the membrane electrode assembly according to claim 1 .

12. A solid polymer electrolyte membrane, in, The solid polymer electrolyte membrane comprises a woven fabric and a fluorine-containing polymer having an ion exchange group. The opening ratio of the woven fabric is more than 50%, The denier of the warp yarn and the denier of the weft yarn constituting the woven fabric are each independently 2 or more, When the thickness of the solid polymer electrolyte membrane is set to Y μm and the ion exchange capacity of the fluorinated polymer is set to X milliequivalents / g of dry resin, the relationship Y≤240X-170 is satisfied. The density of the warp yarns and the weft yarns constituting the woven fabric is more than 150 yarns / inch and less than or equal to 200 yarns / inch.