Bromine-containing compound leveling agent and copper electroplating solution using same

By using fluorene-containing polymers and naphthalimide compounds as leveling agents in copper foil leveling agents, combining the synergistic effects of chloride ions and other additives, the problem of microblind pore filling in the prior art is solved, and the problem of microblind pore filling in the existing technology is achieved. The copper plating effect with high filling rate and low deposition thickness is achieved to meet the manufacturing needs of high-density printed circuit boards.

CN118932438APending Publication Date: 2024-11-12LANZHOU JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410930103.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing copper foil leveling agent cannot achieve high-deep diameter ratio, no gaps, no hole filling in micro-blind holes, and low surface copper thickness, which cannot meet the high density, lightweight, and high integration printed circuit board manufacturing needs. .

Method used

The fluorene-containing polymer and naphthalimide compounds are used as leveling agents to adsorb the copper surface through bromide ions, occupying the adsorption site, and combining the synergistic action of chloride ions and other additives to achieve superfilling of blind pores.

Benefits of technology

Electroplating copper filling with microblind holes with different depth diameter ratios is achieved without holes and seamlessly, with a filling rate of 93 to 97%, a small thickness of copper surface deposition, and the electroplating copper solution has stable properties, long service life and low environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932438A_ABST
    Figure CN118932438A_ABST
Patent Text Reader

Abstract

The invention discloses a bromine-containing compound leveling agent and a copper electroplating solution using the same, and belongs to the technical field of copper foil leveling agents. The bromine-containing compound leveling agent is one of a fluorene-containing polymer or a naphthalimide-containing compound. 1L of the copper electroplating solution using the bromine-containing compound leveling agent is prepared from the following raw materials by weight: 5-250g of copper sulfate pentahydrate; 10 to 100 g of sulfuric acid; 0.001 to 0.5 g of sodium chloride or hydrochloric acid; 0.0001 to 0.05 g of an accelerator; 0.00001 to 0.05 g of a fluorine-containing polymer or a naphthalimide-containing compound, and 0.00001 to 0.05 g of a fluorine-containing 0.005 to 0.8 g of an inhibitor; and adding secondary distilled water to 1L. The copper electroplating solution using the bromine-containing compound leveling agent disclosed by the invention can achieve a better blind hole filling effect. The electroplating copper solution disclosed by the invention has the advantages that the property is stable, and the service life is long; biodegradation is easy, and environmental pollution is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copper foil leveling agents, and in particular relates to a bromine-containing compound leveling agent and a copper electroplating solution using the same. Background Art

[0002] Copper has high resistance to electromigration and low resistivity, and is widely used in copper interconnects of high-density printed circuit boards. Currently, the electroplating solution used for copper in printed circuit boards is mainly copper sulfate solution, and the additives used are mainly divided into three types: inhibitor, accelerator and leveler:

[0003] Among them, the inhibitor is mainly polyethylene glycol (PEG); the leveling agent is mainly quaternary ammonium salts such as Janus green (JGB), diazinon black (DB) or Alcian blue (ABPV), which plays a role in Cu 2+ Competitive adsorption in the high current density area inhibits copper deposition, and the adsorption in the low current area is relatively less; the accelerator, mainly sodium polydisulfide propane sulfonate (SPS) or sodium 3-mercapto-1-propane sulfonate (MPS), is more easily adsorbed in the low current density area; the above three additives work together to form a phenomenon of slow deposition in the high current area and fast deposition in the low current area, thereby achieving the purpose of leveling.

[0004] However, as electronic devices develop towards multifunctionality, high performance, lightness, and compactness, high-density, lightweight, and highly integrated printed circuit boards have become an inevitable demand of the industry. Along with this demand, the width of copper interconnects on printed circuit boards is becoming narrower and narrower, and the seamless and void-free filling of micro blind vias with high aspect ratios and the lower surface copper deposition thickness have become a key issue in the manufacturing technology of copper interconnects on printed circuit boards.

[0005] In the prior art, the leveling agent, for example, JGB, has the following effect on blind hole filling when it is used as a leveling agent on electrolytic copper foil: Figure 4 As shown in the figure, it can be clearly observed that Jiana Green cannot completely fill the micro blind via with a depth-to-diameter ratio of 1:1. Complete filling of the blind via is the prerequisite for realizing the function of the entire circuit, which ensures the electrical connection between layers. If it cannot be completely filled, the circuit function will not be realized, and the actual application of electronic products will not be able to realize the function.

[0006] The inventor's patent ZL201310057889.2 "Electroplating copper solution containing mercapto heterocyclic compounds" discovered and solved the above technical problems, using mercapto heterocyclic compounds to achieve electroplating copper filling of blind microvias with different depth-to-diameter ratios in the electroplating process without voids, gaps, and good leveling effect. On this basis, further exploration is conducted to see if there are other compounds with this function that can achieve similar or better technical effects. Based on this, the researchers proposed a bromine-containing compound leveler and an electroplating copper solution using it. Summary of the invention

[0007] The object of the present invention is to provide a bromine compound leveler and a copper electroplating solution using the same, so as to solve the problem that existing copper foil additives cannot achieve seamless and void-free filling in micro blind holes with high aspect ratio and lower surface copper deposition thickness.

[0008] In order to solve the above problems, the technical solution of the present invention is:

[0009] A bromine-containing compound leveler, which is an electrolytic copper foil leveler containing a fluorene polymer. The fluorene-containing polymer leveler is any one of polyfluorene, poly(9,9-dioctylfluorene-2,7-dione) (PFO), poly(9,9-dioctylfluorene-2,7-diphenylamine) (PFB), poly(9,9-bis{3'-[(N,N-dimethyl)-N-ethylammonium}-propyl]-2,7-fluorene dibromide) (P_B_), poly(9,9-dioctylfluorene) (PFF), poly(dimethoxyfluorene) (POMe), and poly(triacontoxymethoxyfluorene) (PFOMe).

[0010] A bromine-containing compound leveler, the bromine-containing compound leveler is an electrolytic copper foil leveler containing a naphthalene imide compound, the naphthalene imide compound is naphthalene-1,8-dicarboximide (NDI), N-butyl-4-(aza-15-crown-5)-1,8-naphthalene imide (BACN), 4-bromo-N-(2-(N,N-di(2-methoxycarbonylethyl)-amino)ethyl)-1,8-naphthalene imide (BCANM), 2,7-bis(3-(dimethylamino)propyl)benzo(1,3,6,8)phenanthroline-1,3,6,8(2H,7H)-tetraone dibromide (NDI-N-Br), 4-(1-piperidinyl)-1,8-naphthalene anhydride (PNA), 4-(1-piperidinyl)-N-(2-aminoethyl)-1,8-naphthalene imide (PANM), 1-acetyl-8-chloro-4,5-dimethoxynaphthalene imide (ACDMND).

[0011] The copper electroplating solution used in the above-mentioned bromine-containing compound leveler is composed of the following raw materials in the following mass ratios per liter:

[0012] 5-250g of copper sulfate pentahydrate; 10-100g of sulfuric acid; 0.001-0.5g of sodium chloride or hydrochloric acid; 0.0001-0.05g of accelerator; 0.00001-0.05g of fluorene-containing polymer or naphthaleneimide-containing compound; 0.005-0.8g of inhibitor; add double distilled water to 1L.

[0013] Furthermore, 1L of the above copper electroplating solution preferably contains the following raw materials in the following mass ratio:

[0014] 50-250g of copper sulfate pentahydrate; 20-60g of sulfuric acid; 0.02-0.25g of sodium chloride or hydrochloric acid; 0.001-0.03g of accelerator; 0.0001-0.02g of fluorene-containing polymer or naphthaleneimide-containing compound; 0.04-0.4g of inhibitor; add double distilled water to 1L.

[0015] Furthermore, the optimal mass ratio of the raw materials in 1L of the above copper electroplating solution is:

[0016] 220g of copper sulfate pentahydrate; 54g of sulfuric acid; 0.04g of sodium chloride or hydrochloric acid; 0.001g of accelerator; 0.0003g of fluorene-containing polymer or naphthaleneimide-containing compound; 0.2g of inhibitor; add double distilled water to 1L.

[0017] Furthermore, the accelerator is sodium polydisulfide propane sulfonate or sodium 3-mercapto-1-propane sulfonate.

[0018] Furthermore, the inhibitor is one of polyethylene glycol, block polyether or polyvinyl pyrrolidone.

[0019] Furthermore, the polyethylene glycol is any one of PEG-4000 having a number average molecular weight of 4000, PEG-6000 having a number average molecular weight of 6000, or PEG-8000 having a number average molecular weight of 8000.

[0020] Further, the block polyether is any one of Pluronic PE3100 having a number average molecular weight of 1000, Pluronic PE4300 having a number average molecular weight of 1750, Pluronic PE6100 having a number average molecular weight of 2000, Pluronic PE6200 having a number average molecular weight of 2450, Pluronic PE6400 having a number average molecular weight of 2900, Pluronic PE6800 having a number average molecular weight of 8000, Pluronic RPE1740 having a number average molecular weight of 2125, and Pluronic RPE2035 having a number average molecular weight of 3080.

[0021] Furthermore, the polyvinyl pyrrolidone is any one of PVPK30, PVPK16-18, and PVPK23-27.

[0022] The beneficial effects of the present invention are as follows:

[0023] (1) The present invention uses a fluorene-containing polymer as a leveling agent. Its mechanism of action is different from that of conventional leveling agents based on quaternary ammonium salts such as Janus Green (JGB), Diazine Black (DB) or Alcian Blue (ABPV) in the following ways:

[0024] When organic dye substances such as JGB are used as leveling agents, the main functional group is -N=N-. The present invention introduces fluorene-containing polymers and naphthalene imide compounds originally used in the field of corrosion inhibitors into the field of leveling agents. Its functional groups are completely different from those of traditional leveling agents such as Figure 4 As shown in the Fukui function, the main active components of fluorene-containing polymers and naphthylimide-containing compounds are the bromine Br4 and Br6 therein. The mechanism of action is that bromide ions are adsorbed onto the copper surface, thereby occupying the adsorption sites on the copper surface and inhibiting the deposition of copper ions. The super-filling of blind holes is finally achieved through the synergistic effect with chloride ions and the other two additives.

[0025] At the same time, according to DFT theoretical calculation and simulation research, such as Figure 4 As shown, the functional groups of the traditional leveler JGB are N11 and N21; the functional group in ZL201310057889.2 "Electroplating copper solution containing mercapto heterocyclic compounds" is S7; and the fluorene-containing polymer P_B and the naphthylimide-containing compound N_D in the present invention can play a substitution role, and the active group S7 of the mercapto heterocyclic compound 2-MP is replaced by Br4 to achieve a similar functional role.

[0026] (2) On this basis, the present invention selects sodium polydisulfide propane sulfonate or 3-mercapto-1-propane sulfonate as an accelerator, polyethylene glycol, block polyether or polyvinyl pyrrolidone as an inhibitor, and cooperates with chloride ions. The four additives achieve filling through synergistic effect during the copper plating process. The specific synergistic process is as follows:

[0027] The synergistic effect of polyethylene glycol (PEG) and chloride ions is manifested in that when there is no chloride ion, PEG has a weak cathodic polarization effect. When there is chloride ion, chloride ion is the anchor point of PEG. - , Cu + Formation of PEG–Cu on copper surface + –Cl - Complex film;

[0028] The synergistic effect between sodium poly(disulfide propane sulfonate) (SPS) and chloride ions is manifested in that SPS increases cathode polarization and inhibits copper deposition in the absence of chloride ions. When chloride ions are present, SPS exhibits a depolarizing effect, thereby accelerating copper deposition. In addition, there is competitive adsorption between PEG and SPS, and SPS replaces PEG–Cu + –Cl - The PEG adsorbed on the complex film accelerates the reduction of copper ions.

[0029] Fluorene-containing polymer P_B and PEG can generate a composite inhibitor PEG-P_B, thereby strengthening the inhibitory effect of PEG, and the inhibitory effect of PEG-P_B is sensitive to the convection intensity, and the inhibitory ability under strong convection is stronger than that under weak convection. The copper deposition rate under strong convection is lower than that under weak convection, so increasing the convection intensity difference between the inside and outside of the blind hole is conducive to super filling of the blind hole and further realizing bottom-up filling. At the same time, the free ion Br4 is adsorbed to the copper interface, thereby occupying the adsorption site on the copper surface, thereby inhibiting the deposition of copper ions.

[0030] The mechanism of action of naphthalene-containing imide compounds is similar to that of fluorene-containing polymers. They mainly absorb free bromide ions Br6 onto the copper surface and occupy adsorption sites, thereby inhibiting the deposition of copper ions.

[0031] (3) The fluorene-containing polymer and the naphthalene-containing imide compound selected in the present invention were originally used as rust inhibitors in the field of steel corrosion. In the present invention, they are creatively introduced into the leveling agent in the field of electrolytic copper foil, and are used in the electroplating solution in combination with the above-mentioned accelerator, inhibitor and other additives, so as to achieve electroplated copper filling of blind micro-holes with different aspect ratios without voids, gaps and good leveling effect. Compared with the mercapto-containing heterocyclic compound 2-MP, by calculating the filling rate (FP=H1 / H2×100%), it can be obtained that the filling rates of the fluorene-containing polymer (97.6%, Example 13) and the naphthalene-containing imide compound (98.7%, Example 27) are both greater than 2-MP (90%), and the copper surface deposition thickness is small and the filling rate is higher. Figure 5-7 It can be clearly seen from the comparison that the copper electroplating solution using the bromine-containing compound leveler disclosed in the present invention can achieve a better blind hole filling effect. It can reach 93-97% or more. The copper electroplating solution of the present invention has stable properties and long service life; it is easy to biodegrade and has little environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is the polarization characteristic curve of Janus Green (JGB);

[0033] Figure 2 is the polarization characteristic curve of fluorene-containing polymer (P_B);

[0034] Figure 3 is the polarization characteristic curve of naphthalene imide compound (N_D);

[0035] Figure 4 It is the Fukui function diagram of Janus green (JGB), thiol-containing heterocyclic compound (2-MP), fluorene-containing polymer (P_B), and naphthalene imide-containing compound (N_D);

[0036] Figure 5This is a blind hole filling effect diagram of a mercapto heterocyclic compound (2-MP) disclosed in China ZL201310057889.2 "Electroplating copper solution containing mercapto heterocyclic compounds";

[0037] Figure 6 This is the blind hole filling effect diagram when the fluorene-containing polymer (P_B) is used as a leveling agent;

[0038] Figure 7 This is a diagram of the blind hole filling effect when using naphthaleneimide compounds (N_D) as leveling agents. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention as claimed but is merely representative of selected embodiments of the present invention.

[0041] A bromine-containing compound leveler, which is an electrolytic copper foil leveler containing a fluorene polymer (P_B), and the fluorene polymer leveler is any one of polyfluorene, poly(9,9-dioctylfluorene-2,7-dione) (PFO), poly(9,9-dioctylfluorene-2,7-diphenylamine) (PFB), poly(9,9-bis{3'-[(N,N-dimethyl)-N-ethylammonium}-propyl]-2,7-fluorene dibromide) (P_B_), poly(9,9-dioctylfluorene) (PFF), poly(dimethoxyfluorene) (POMe), and poly(triacontoxymethoxyfluorene) (PFOMe).

[0042] Another bromine-containing compound leveler is an electrolytic copper foil leveler containing a naphthalene imide compound (N_D), wherein the naphthalene imide compound is naphthalene-1,8-dicarboximide (NDI), N-butyl-4-(aza-15-crown-5)-1,8-naphthalene imide (BACN), 4-bromo-N-(2-(N,N-di(2-methoxycarbonylethyl)-amino)ethyl)-1,8-naphthalene Any one of imide (BCANM), 2,7-bis(3-(dimethylamino)propyl)benzo(1,3,6,8)phenanthroline-1,3,6,8(2H,7H)-tetraone dibromide (NDI-N-Br), 4-(1-piperidinyl)-1,8-naphthalene anhydride (PNA), 4-(1-piperidinyl)-N-(2-aminoethyl)-1,8-naphthalene imide (PANM), and 1-acetyl-8-chloro-4,5-dimethoxynaphthalene imide (ACDMND).

[0043] The copper electroplating solution using the above two categories of bromine-containing compound levelers, 1L of the copper electroplating solution is composed of the following raw materials in the following mass ratio: 5-250g of copper sulfate pentahydrate; 10-100g of sulfuric acid; 0.001-0.5g of sodium chloride or hydrochloric acid; 0.0001-0.05g of accelerator; 0.00001-0.05g of leveler, i.e., fluorene-containing polymer (P_B) or naphthaleneimide-containing compound (N_D); 0.005-0.8g of inhibitor; and double distilled water is added to 1L.

[0044] Example 1 (Please check and verify the data of Examples 1-28 carefully to see if they are consistent with the large table. Be sure to check carefully) Electroplating copper solution using bromine-containing compound leveler, 1L of the electroplating copper solution is composed of the following raw materials in the following mass ratio:

[0045] Copper sulfate pentahydrate 15g;

[0046] Sulfuric acid 20g

[0047] Hydrochloric acid 0.004g

[0048] Accelerator, in this example, 0.025g sodium polydisulfide dipropane sulfonate Leveler, in this example, 0.05g polyfluorene

[0049] Inhibitor, in this example PEG4000, 0.02 g

[0050] Add double distilled water to 1L.

[0051] Example 2

[0052] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0053] Copper sulfate pentahydrate 100g;

[0054] Sulfuric acid 15g

[0055] Hydrochloric acid 0.02g

[0056] Accelerator, in this embodiment, 0.002 g of sodium 3-mercapto-1-propane sulfonate;

[0057] Leveling agent, in this embodiment, poly (9,9-dioctylfluorene-2,7-dione) (PFO) 0.025 g;

[0058] Inhibitor, in this example PEG-6000, 0.3 g;

[0059] Add double distilled water to 1L.

[0060] Example 3

[0061] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0062] Copper sulfate pentahydrate 45g;

[0063] Sulfuric acid 40g;

[0064] Hydrochloric acid 0.003 g;

[0065] Accelerator, in this embodiment, 0.0001 g of sodium 3-mercapto-1-propane sulfonate;

[0066] Leveling agent, in this embodiment, poly (9,9-dioctylfluorene-2,7-diylaniline) (PFB) 0.00001 g;

[0067] Inhibitor, in this example, PEG8000, 0.003 g;

[0068] Add double distilled water to 1L.

[0069] Example 4

[0070] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0071] Copper sulfate pentahydrate 50g;

[0072] 50g sulfuric acid;

[0073] Hydrochloric acid 0.05 g;

[0074] Accelerator, in this embodiment, 0.0001 g of sodium polydisulfide dipropane sulfonate;

[0075] Leveling agent, in this embodiment, poly (9,9-bis {3'-[(N,N-dimethyl)-N-ethylammonium}-propyl]-2,7-fluorene dibromide) (P_B) 0.05g;

[0076] Inhibitor, in this embodiment, Pluronic PE3100, 0.4 g;

[0077] Add double distilled water to 1L.

[0078] Example 5

[0079] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0080] Copper sulfate pentahydrate 100g;

[0081] 90g sulfuric acid;

[0082] Hydrochloric acid 0.001 g;

[0083] Accelerator, in this embodiment, 0.0003 g of sodium polydisulfide dipropane sulfonate;

[0084] Leveling agent, in this embodiment, poly (9,9-dioctylfluorene) (PFF) 0.0002 g;

[0085] Inhibitor, in this embodiment, Pluronic PE4300, 0.01 g;

[0086] Add double distilled water to 1L.

[0087] Example 6

[0088] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0089] Copper sulfate pentahydrate 110g;

[0090] Sulfuric acid 10g;

[0091] Hydrochloric acid 0.002 g;

[0092] Accelerator, in this embodiment, 0.0003 g of sodium 3-mercapto-1-propane sulfonate;

[0093] Leveling agent, in this embodiment, poly(dimethoxyfluorene) (POMe) 0.0003 g;

[0094] Inhibitor, in this embodiment, Pluronic PE6100, 0.008 g;

[0095] Add double distilled water to 1L.

[0096] Example 7

[0097] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0098] Copper sulfate pentahydrate 74g;

[0099] Sulfuric acid 35g;

[0100] Sodium chloride 0.003 g;

[0101] Accelerator, in this embodiment, 0.01 g of sodium polydisulfide dipropane sulfonate;

[0102] Leveling agent, in this embodiment, poly(triacontaethoxymethoxyfluorene) (PFOMe) 0.002 g;

[0103] Inhibitor, in this embodiment, Pluronic PE6200, 0.015 g;

[0104] Add double distilled water to 1L.

[0105] Example 8

[0106] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0107] Copper sulfate pentahydrate 30g;

[0108] Sulfuric acid 75g;

[0109] Sodium chloride 0.06 g;

[0110] Accelerator, sodium 3-mercapto-1-propane sulfonate 0.05 g;

[0111] Leveling agent, in this embodiment, poly(triacontaethoxymethoxyfluorene) (PFOMe) 0.0003 g;

[0112] Inhibitor, in this embodiment, Pluronic PE6400, 0.02 g;

[0113] Add double distilled water to 1L.

[0114] Example 9

[0115] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0116] Copper sulfate pentahydrate 15g;

[0117] Sulfuric acid 45g;

[0118] Sodium chloride 0.006 g;

[0119] Accelerator, in this embodiment, 0.002 g of sodium polydisulfide dipropane sulfonate;

[0120] Leveling agent, in this embodiment, poly (9,9-dioctylfluorene-2,7-dione) (PFO) 0.003 g;

[0121] Inhibitor, in this embodiment, Pluronic PE6800, 0.02 g;

[0122] Add double distilled water to 1L.

[0123] Example 10

[0124] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0125] Copper sulfate pentahydrate 250g;

[0126] Sulfuric acid 100g;

[0127] Sodium chloride 0.25 g;

[0128] Accelerator, in this embodiment, 0.025 g of sodium 3-mercapto-1-propane sulfonate;

[0129] Leveling agent, in this embodiment, poly (9,9-bis {3'-[(N,N-dimethyl)-N-ethylammonium}-propyl]-2,7-fluorene dibromide) (P_B) 0.025g;

[0130] Inhibitor, in this example, Pluronic RPE1740, 0.005 g;

[0131] Add double distilled water to 1L.

[0132] Embodiment 11

[0133] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0134] Copper sulfate pentahydrate 200g;

[0135] Sulfuric acid 23g;

[0136] Sodium chloride 0.02 g;

[0137] Accelerator, in this embodiment, 0.05 g of sodium polydisulfide dipropane sulfonate;

[0138] Leveling agent, in this embodiment, poly (9,9-dioctylfluorene-2,7-diylaniline) (PFB) 0.0025 g;

[0139] Inhibitor, in this example, Pluronic RPE2035, 0.3 g;

[0140] Add double distilled water to 1L.

[0141] Example 12

[0142] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0143] Copper sulfate pentahydrate 170g;

[0144] Sulfuric acid 10g;

[0145] Sodium chloride 0.1 g;

[0146] Accelerator, in this embodiment, 0.004 g of sodium 3-mercapto-1-propane sulfonate;

[0147] Leveling agent, in this embodiment, poly (9,9-dioctylfluorene) (PFF) 0.003 g;

[0148] Inhibitor, in this example PVPK30, 0.02 g;

[0149] Add double distilled water to 1L.

[0150] Embodiment 13

[0151] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0152] Copper sulfate pentahydrate 130g;

[0153] 50g sulfuric acid;

[0154] Sodium chloride 0.007 g;

[0155] Accelerator, in this embodiment, 0.03 g of sodium polydisulfide dipropane sulfonate;

[0156] Leveling agent, in this embodiment, poly(dimethoxyfluorene) (POMe) 0.02 g;

[0157] Inhibitor, in this example PVPK16-18, 0.02 g;

[0158] Add double distilled water to 1L.

[0159] Embodiment 14

[0160] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0161] Copper sulfate pentahydrate 35g;

[0162] Sulfuric acid 35g;

[0163] Sodium chloride 0.2g;

[0164] Accelerator, in this embodiment, 0.0003 g of sodium 3-mercapto-1-propane sulfonate;

[0165] Leveling agent, in this embodiment, 0.0035 g of polyfluorene;

[0166] Inhibitor, in this example PVPK23-27, 0.02 g;

[0167] Add double distilled water to 1L.

[0168] Embodiment 15

[0169] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0170] Copper sulfate pentahydrate 10g;

[0171] Sulfuric acid 5g;

[0172] Sodium chloride 0.02 g;

[0173] Accelerator, in this embodiment, 0.01 g of sodium polydisulfide dipropane sulfonate;

[0174] Leveling agent, in this embodiment, 0.001 g of naphthalene imide (N_D);

[0175] Inhibitor, in this example, PEG4000, 0.006 g;

[0176] Add double distilled water to 1L.

[0177] Example 16

[0178] The copper electroplating solution used as a bromine compound leveler, 1L of the copper electroplating solution is composed of the following raw materials in the following mass ratios: 25g of copper sulfate pentahydrate;

[0179] Sulfuric acid 10g;

[0180] Sodium chloride 0.1 g;

[0181] Accelerator, in this embodiment, 0.0001 g of sodium 3-mercapto-1-propane sulfonate;

[0182] Leveling agent, in this example, 0.0003 g of N-butyl-4-(aza-15-crown-5)-1,8-naphthaleneimide (BACN);

[0183] Inhibitor, in this example, PEG6000, 0.01 g;

[0184] Add double distilled water to 1L.

[0185] Embodiment 17

[0186] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0187] Copper sulfate pentahydrate 5g;

[0188] 50g sulfuric acid;

[0189] Sodium chloride 0.003 g;

[0190] Accelerator, in this embodiment, 0.015 g of sodium 3-mercapto-1-propane sulfonate;

[0191] Leveling agent, in this embodiment, 4-bromo-N-(2-(N,N-bis(2-methoxycarbonylethyl)-amino)ethyl)-1,8-naphthaleneimide (BCANM) 0.02 g;

[0192] Inhibitor, in this example, PEG8000, 0.35 g;

[0193] Add double distilled water to 1L.

[0194] Embodiment 18

[0195] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0196] Copper sulfate pentahydrate 50g;

[0197] Sulfuric acid 20g;

[0198] Sodium chloride 0.001 g;

[0199] Accelerator, in this embodiment, 0.025 g of sodium polydisulfide dipropane sulfonate;

[0200] Leveling agent, in this embodiment, 0.004 g of 2,7-bis(3-(dimethylamino)propyl)benzo(1,3,6,8)phenanthroline-1,3,6,8(2H,7H)-tetraone dibromide (NDI-N-Br);

[0201] Inhibitor, in this embodiment, Pluronic PE3100, 0.45 g;

[0202] Add double distilled water to 1L.

[0203] Embodiment 19

[0204] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0205] Copper sulfate pentahydrate 40g;

[0206] Sulfuric acid 15g;

[0207] Sodium chloride 0.004 g;

[0208] Accelerator, in this embodiment, 0.02 g of sodium 3-mercapto-1-propane sulfonate;

[0209] Leveling agent, in this embodiment, 4-(1-piperidinyl)-1,8-naphthalene anhydride (PNA), 4-(1-piperidinyl)-N-(2-aminoethyl)-1,8-naphthalene imide (PANM) 0.03 g;

[0210] Inhibitor, in this embodiment, Pluronic PE4300, 0.2 g;

[0211] Add double distilled water to 1L.

[0212] Embodiment 20

[0213] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0214] Copper sulfate pentahydrate 235g;

[0215] 70g of sulfuric acid;

[0216] Sodium chloride 0.12 g;

[0217] Accelerator, in this embodiment, 0.003 g of sodium polydisulfide dipropane sulfonate;

[0218] Leveling agent, in this embodiment, 0.002 g of 1-acetyl-8-chloro-4,5-dimethoxynaphthalimide (ACDMND);

[0219] Inhibitor, in this example, Pluronic PE6100, 0.5 g;

[0220] Add double distilled water to 1L.

[0221] Embodiment 21

[0222] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0223] Copper sulfate pentahydrate 125g;

[0224] Sulfuric acid 40g;

[0225] Sodium chloride 0.5 g;

[0226] Accelerator, in this embodiment, 0.025 g of sodium 3-mercapto-1-propane sulfonate;

[0227] Leveling agent, in this embodiment, 0.0004 g of naphthalene imide (N_D);

[0228] Inhibitor, in this embodiment, Pluronic PE6200, 0.35 g;

[0229] Add double distilled water to 1L.

[0230] Embodiment 22

[0231] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0232] Copper sulfate pentahydrate 100g;

[0233] 50g sulfuric acid;

[0234] Hydrochloric acid 0.004 g;

[0235] Accelerator, in this embodiment, 0.0001 g of sodium polydisulfide dipropane sulfonate;

[0236] Leveling agent, in this example, 0.015 g of N-butyl-4-(aza-15-crown-5)-1,8-naphthaleneimide (BACN);

[0237] Inhibitor, in this embodiment, Pluronic PE6400, 0.004 g;

[0238] Add double distilled water to 1L.

[0239] Embodiment 23

[0240] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0241] Copper sulfate pentahydrate 70g;

[0242] Sulfuric acid 100g;

[0243] Hydrochloric acid 0.02 g;

[0244] Accelerator, in this embodiment, 0.003 g of sodium 3-mercapto-1-propane sulfonate;

[0245] Leveling agent, in this embodiment, 0.003 g of 2,7-bis(3-(dimethylamino)propyl)benzo(1,3,6,8)phenanthroline-1,3,6,8(2H,7H)-tetraone dibromide (NDI-N-Br);

[0246] Inhibitor, in this embodiment, Pluronic PE6800, 0.8 g;

[0247] Add double distilled water to 1L.

[0248] Embodiment 24

[0249] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0250] Copper sulfate pentahydrate 250g;

[0251] Sulfuric acid 80g;

[0252] Hydrochloric acid 0.15 g;

[0253] Accelerator, in this embodiment, 0.04 g of sodium polydisulfide dipropane sulfonate;

[0254] Leveling agent, in this embodiment, 4-bromo-N-(2-(N,N-bis(2-methoxycarbonylethyl)-amino)ethyl)-1,8-naphthaleneimide (BCANM) 0.006 g;

[0255] Inhibitor, in this example, Pluronic RPE1740, 0.75 g;

[0256] Add double distilled water to 1L.

[0257] Embodiment 25

[0258] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0259] Copper sulfate pentahydrate 60g;

[0260] Sulfuric acid 20g;

[0261] Hydrochloric acid 0.36 g;

[0262] Accelerator, in this embodiment, 0.0025 g of sodium 3-mercapto-1-propane sulfonate;

[0263] Leveling agent, in this embodiment, 0.003 g of naphthalene imide (N_D);

[0264] Inhibitor, in this example, Pluronic RPE2035, 0.25 g;

[0265] Add double distilled water to 1L.

[0266] Embodiment 26

[0267] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0268] Copper sulfate pentahydrate 45g;

[0269] Sulfuric acid 75g;

[0270] Hydrochloric acid 0.13 g;

[0271] Accelerator, in this embodiment, 0.05 g of sodium polydisulfide dipropane sulfonate;

[0272] Leveling agent, in this embodiment, 4-(1-piperidinyl)-1,8-naphthalene anhydride (PNA), 4-(1-piperidinyl)-N-(2-aminoethyl)-1,8-naphthalene imide (PANM), 0.05 g;

[0273] Inhibitor, in this example PVPK30, 0.10 g;

[0274] Add double distilled water to 1L.

[0275] Embodiment 27

[0276] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0277] Copper sulfate pentahydrate 110g;

[0278] Sulfuric acid 30g;

[0279] Hydrochloric acid 0.25 g;

[0280] Accelerator, in this embodiment, 0.03 g of sodium polydisulfide dipropane sulfonate;

[0281] Leveling agent, in this embodiment, 0.007 g of 1-acetyl-8-chloro-4,5-dimethoxynaphthalimide (ACDMND);

[0282] Inhibitor, in this example PVPK16-18, 0.35 g;

[0283] Add double distilled water to 1L.

[0284] Embodiment 28

[0285] The copper electroplating solution used for the bromine compound leveler is composed of the following raw materials in the following mass ratios:

[0286] Copper sulfate pentahydrate 10g;

[0287] Sulfuric acid 60g;

[0288] Hydrochloric acid 0.4 g;

[0289] Accelerator, in this embodiment, 0.004 g of sodium 3-mercapto-1-propane sulfonate;

[0290] Leveling agent, in this example, 0.025 g of N-butyl-4-(aza-15-crown-5)-1,8-naphthaleneimide (BACN);

[0291] Inhibitor, in this example PVPK23-27, 0.65 g;

[0292] Add double distilled water to 1L.

[0293] Preparation of electroplating copper solution using the above two types of bromine-containing levelers:

[0294] According to the mass ratio of each raw material in Example 1-Example 28, add copper sulfate pentahydrate to a beaker, add 900mL of secondary distilled water until the copper sulfate pentahydrate is completely dissolved, then add sulfuric acid, and wait until it is completely dissolved and the solution temperature drops to room temperature. According to the copper electroplating solution formula listed in Examples 1-28, add inhibitors, accelerators and levelers in sequence, stir evenly, then add sodium chloride or hydrochloric acid, and dilute to 1L with secondary deionized water to ensure that the chloride ion concentration in the electroplating solution is 0.04g / L. The above solution diluted to 1L is the electroplating solution mother solution.

[0295] The quality of the above-mentioned electroplating solution mother solution can be judged by the following three methods. The specific steps are as follows:

[0296] 1. Fill rate;

[0297] The quality of the electroplating mother solution is judged by electroplating, and the filling result is evaluated by the filling performance (FP), and the filling effect obtained by the electroplating solution used is calculated. The evaluation standard is the calculated filling rate. In the above embodiments, Example 1, Example 5, Example 13, Example 15, Example 21, and Example 27 are randomly selected for calculation, and the calculation results of the filling rate are as follows:

[0298] Table 1: Filling rate of some examples

[0299]

[0300]

[0301] As shown in Table 1, the filling rates of some randomly selected embodiments are all above 97%. At the molecular level, the active sites and functional groups of JGB, 2-MP, fluorene-containing polymers (P_B), naphthalene imide compounds (N_D) with inhibitors and accelerators in the presence of chloride ions are revealed to achieve blind hole filling. At the same time, it fills the gap in the DFT theory of the functional group mechanism in Chinese patent ZL201310057889.2 "Electroplating copper solution containing thiol heterocyclic compounds". And the filling rate and filling performance of the embodiments disclosed in the present invention are significantly higher than the results published in Chinese patent ZL201310057889.2 "Electroplating copper solution containing thiol heterocyclic compounds".

[0302] 2. Micro blind hole electroplating filling test;

[0303] After electroplating, the parts are polished on a metallographic polishing machine, and during this period, they are observed and photographed with a metallographic microscope of different magnifications for comparison.

[0304] The electroplating solutions prepared in Example 13 and Example 27 of the present invention and the electroplating solution with an equal amount of Janus Green added as a leveling agent were selected to electroplate and fill the above-mentioned rectangular samples of 20 mm×40 mm according to the conventional electroplating copper process, and the cross sections of the samples were photographed with a metallographic microscope. The photographs taken are shown in FIG. Figure 6 and Figure 7 , in contrast to Figure 4 This is a blind hole filling effect diagram of a mercapto heterocyclic compound (2-MP) disclosed in Chinese patent ZL201310057889.2 "Electroplating copper solution containing mercapto heterocyclic compounds".

[0305] For a micro blind hole with a depth-to-diameter ratio of 1:1, under the same electroplating conditions:

[0306] When filling micro blind holes with mercapto heterocyclic compounds (2-MP) disclosed in Chinese patent ZL201310057889.2 "Electroplating copper solution containing mercapto heterocyclic compounds", such as Figure 5 As shown, the strong inhibitory effect of 2-MP means that no matter how the ratio of the additives in the copper electroplating solution is changed, 100% filling or bump filling cannot be achieved, which poses a great challenge to the multi-layer packaging between printed circuits in the future.

[0307] When the present invention uses the fluorene-containing polymer (P_B) and the naphthalene imide-containing compound (N_D) as the leveling agent, the effect of using it in the copper electroplating solution is as follows: Figure 5 and Figure 7 It can be seen that perfect filling of micro blind holes can be achieved, and it is clearly seen from the figure that on the basis of achieving defect-free filling of electroplated copper micro blind holes, the copper layer deposition thickness is not only less than 10μm, but also the blind holes achieve 100% super filling, and the blind hole filling has an obvious convex effect, which lays a foundation for multi-layer stacking between multi-layer printed circuits and improving the performance and reliability of printed circuit boards.

[0308] 3. Electrochemical characteristic test;

[0309] In order to verify that the fluorene-containing polymer (P_B) and the naphthalene imide-containing compound (N_D) selected in the present invention as a leveler can be used in the copper electroplating solution to replace the traditional Janus Green (JGB) and the thiol-containing heterocyclic compound (2-MP) disclosed in Chinese Patent ZL201310057889.2 "Electroplating copper solution containing thiol heterocyclic compound", the inventors conducted a large number of comparative tests, and only selected representative electrochemical characteristic tests and micro blind hole electroplating filling experiments for public comparison. The specific process is as follows:

[0310] Add water to 100mL in the proportion of 10g copper sulfate pentahydrate, 5g sulfuric acid, and 0.0004g hydrochloric acid (since the accelerator, leveler, and inhibitor in this experiment are in the ppm level, all substances in the formula should be dissolved to 100mL. In this laboratory, copper sulfate pentahydrate, sulfuric acid, and hydrochloric acid are first dissolved to 100mL and then a trace amount of accelerator, leveler, and inhibitor is added, which will not affect the experimental results). The rotation speeds of the rotating disk electrode are 100rpm and 1000rpm respectively, and the temperature is 25±3℃. Polyfluorene and naphthaleneimide are used as levelers to measure whether they have convection-dependent adsorption characteristic behavior, and compared with the commonly used Janus green as a leveler. Specifically:

[0311] When the electrode of the electrochemical workstation (Reference 6200, Gamry) was working for 500 s, a 200 ppm inhibitor PE4300 solution was injected;

[0312] When the electrode worked for 1000 s, 1 ppm of sodium 3-mercapto-1-propane sulfonate was injected as an accelerator;

[0313] When the electrode was working for 2000s, 1ppm of Jiana Green was injected and data was collected. Figure 1 Electrochemical behavior characteristic curve.

[0314] Similarly, in the other two experiments:

[0315] When the electrode was working for 3000s, 1ppm polyfluorene and 1ppm naphthaleneimide were injected respectively and data were collected. Figure 2 and Figure 3 curve, Figure 2 and Figure 3 The characteristic curves respectively represent the synergistic competitive effects between polyfluorene and naphthalene imide and the inhibitor PE4300, the accelerator sodium 3-mercapto-1-propane sulfonate and chloride ion.

[0316] and Figure 1 In contrast, when the rotating disk electrode was operated for 3000s, 1ppm of polyfluorene and 1ppm of naphthalene imide were injected, and the cathode potential shifted negatively, indicating that the fluorene polymer (P_B) and the naphthalene imide compound (N_D) and JGB had similar inhibitory effects on copper deposition. Moreover, after adding 1ppm of polyfluorene and 1ppm of naphthalene imide, the electrochemical behavior characteristics of the fluorene polymer (P_B) compound and the naphthalene imide compound (N_D) under different convection intensities showed a positive potential difference, further verifying that the fluorene polymer (P_B) compound and the naphthalene imide compound (N_D) and the other three added molecules have the same synergistic competitive adsorption behavior as JGB and the other three additive molecules.

[0317] Therefore, the fluorene polymer (P_B) compound and the naphthalene imide compound (N_D) have the function of being a leveler molecule in the electroplating copper blind hole filling plating solution, and P_B can be used as a leveler in the electroplating solution for filling micro blind holes.

Claims

1. A bromine-containing compound leveler, characterized in that: The bromine-containing compound leveling agent is an electrolytic copper foil leveling agent containing a fluorene polymer, and the fluorene-containing polymer leveling agent is any one of polyfluorene, poly(9,9-dioctylfluorene-2,7-dione), poly(9,9-dioctylfluorene-2,7-diphenylamine), poly(9,9-bis{3'-[(N,N-dimethyl)-N-ethylammonium}-propyl]-2,7-fluorene dibromide, poly(9,9-dioctylfluorene), poly(dimethoxyfluorene), and poly(triacontoxymethoxyfluorene).

2. A bromine-containing compound leveler, characterized in that: The bromine-containing compound leveler is an electrolytic copper foil leveler containing a naphthalene imide compound, wherein the naphthalene imide compound is any one of naphthalene imide, N-butyl-4-(aza-15-crown-5)-1,8-naphthalene imide, 4-bromo-N-(2-(N,N-di(2-methoxycarbonylethyl)-amino)ethyl)-1,8-naphthalene imide, 2,7-bis(3-(dimethylamino)propyl)benzo(1,3,6,8)phenanthroline-1,3,6,8(2H,7H)-tetraketone dibromide, 4-(1-piperidinyl)-1,8-naphthalene anhydride (PNA), 4-(1-piperidinyl)-N-(2-aminoethyl)-1,8-naphthalene imide, and 1-acetyl-8-chloro-4,5-dimethoxynaphthalene imide.

3. A copper electroplating solution using a bromine-containing compound leveler, characterized in that: 1L of the copper electroplating solution is composed of the following raw materials in the following mass ratios: 5-250g of copper sulfate pentahydrate; 10-100g of sulfuric acid; 0.001-0.5g of sodium chloride or hydrochloric acid; 0.0001-0.05g of accelerator; 0.00001-0.05g of fluorene-containing polymer or naphthaleneimide-containing compound; 0.005-0.8g of inhibitor; add double distilled water to 1L.

4. The copper electroplating solution using a bromine-containing compound leveler as claimed in claim 3, characterized in that: 1L of the above copper electroplating solution preferably has the following raw materials in the following mass ratio: 50-250g of copper sulfate pentahydrate; 20-60g of sulfuric acid; 0.02-0.25g of sodium chloride or hydrochloric acid; 0.001-0.03g of accelerator; 0.0001-0.02g of fluorene-containing polymer or naphthaleneimide-containing compound; 0.04-0.4g of inhibitor; add double distilled water to 1L.

5. The copper electroplating solution using a bromine-containing compound leveler as claimed in claim 4, characterized in that: The optimal mass ratio of the raw materials in 1L of the above copper electroplating solution is: 220g of copper sulfate pentahydrate; 54g of sulfuric acid; 0.04g of sodium chloride or hydrochloric acid; 0.001g of accelerator; 0.0003g of fluorene-containing polymer or naphthaleneimide-containing compound; 0.2g of inhibitor; add double distilled water to 1L.

6. A copper electroplating solution using a bromine-containing compound leveler as claimed in claims 3-5, characterized in that: The accelerator is sodium polydisulfide dipropane sulfonate or sodium 3-mercapto-1-propane sulfonate.

7. The copper electroplating solution using a bromine-containing compound leveler as claimed in claim 6, characterized in that: The inhibitor is one of polyethylene glycol, block polyether or polyvinyl pyrrolidone.

8. The copper electroplating solution using a bromine-containing compound leveler as claimed in claim 7, characterized in that: The polyethylene glycol is any one of PEG-4000 with a number average molecular weight of 4000, PEG-6000 with a number average molecular weight of 6000, or PEG-8000 with a number average molecular weight of 8000.

9. A copper electroplating solution using a bromine-containing compound leveler as claimed in claim 8, characterized in that: The block polyether is any one of Pluronic PE3100 with a number average molecular weight of 1000, Pluronic PE4300 with a number average molecular weight of 1750, Pluronic PE6100 with a number average molecular weight of 2000, Pluronic PE6200 with a number average molecular weight of 2450, Pluronic PE6400 with a number average molecular weight of 2900, Pluronic PE6800 with a number average molecular weight of 8000, Pluronic RPE1740 with a number average molecular weight of 2125, and Pluronic RPE2035 with a number average molecular weight of 3080.

10. The copper electroplating solution using a bromine-containing compound leveler as claimed in claim 7, characterized in that: The polyvinyl pyrrolidone is any one of PVPK30, PVPK16-18, and PVPK23-27.